MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Outokumpu 353MA® High Temperature Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Alloy with higher nickel content than the other steels. Has increased silicon and nitrogen contents and is microalloyed with rare earth metals (REM). Max service temperature in air is 1150°C, but after service below ~950°C there is a risk for reduced room temperature impact toughness.

Applications: Heat and creep resistance. For use over 550°C for equipment and components within:

  • Iron, steel, and non-ferrous industries
  • Engineering industry
  • Energy conservation plants
  • Cement industry

Available in hot rolled plate (Quarto) form.

Key Words: EN 1.4854; UNS S35315
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.90 g/ccRT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 720 MPaOutokumpu Typical, Hot Rolled Strip/Sheet (CPP); EN 10002-1
Tensile Strength, Yield 360 MPa
@Strain 0.2 %
Outokumpu Typical,Hot rolled Strip/Sheet (CPP); EN 10002-1
 400 MPa
@Strain 1 %
Outokumpu Typical,Hot rolled Strip/Sheet (CPP); EN 10002-1
Elongation at Break 50 %Outokumpu Typical, Hot Rolled Strip/Sheet (CPP); EN 10002-1
Rupture Strength 4.50 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
 8.00 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
 15.0 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
 20.0 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
 28.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
 39.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
 56.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
 82.0 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
 127 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
 206 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
Modulus of Elasticity 190 GPaRT
 130 GPa
@Temperature 1000 °C
 160 GPa
@Temperature 500 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000100 ohm-cmRT
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.6 µm/m-°C
@Temperature 500 °C
 18.2 µm/m-°C
@Temperature 1000 °C
Specific Heat Capacity 0.450 J/g-°CRT
 0.580 J/g-°C
@Temperature 500 °C
Thermal Conductivity 11.3 W/m-KRT
 18.5 W/m-K
@Temperature 500 °C
 26.0 W/m-K
@Temperature 1000 °C
Maximum Service Temperature, Air 1150 °CDry Air
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 1010 - 1040 °CStress Relief Annealing (min. 0.5 h)
 1100 - 1150 °CSolution Annealing
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.050 %
Cerium, Ce 1.3 %
Chromium, Cr 25 %
Iron, Fe 37.18 %
Nickel, Ni 35 %
Nitrogen, N 0.17 %
Silicon, Si 1.3 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Outokumpu 254 SMO® High Performance Austenitic Stainless Steel
Crucible Steel SUE52 Martensitic Steel
Outokumpu 253MA® High Temperature Austenitic Stainless Steel
Outokumpu 4438 High Performance Austenitic Stainless Steel
Outokumpu 4833 High Temperature Austenitic Stainless Steel

NOUTOK48 / 18763

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.