MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
BRP Manufacturing BG625 – Style 406 Nitrile Rubber Sheet – Ultra Strength
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Material: Nitrile Rubber Sheet – Ultra Strength
BRP Style: BG625 – Style 406
Finish: Smooth
ASTM Callout: ASTM D2000 2BG625A14B14B34EF11EF21EO14EO34F17

Information provided by BRP Manufacturing Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength >= 2500 psiOriginal; ASTM D412
 <= 1000 psi
@Temperature 23.0 °C,
Time 252000 sec
EF21 Fluid Resistance, Fuel b; ASTM D471
 <= 1375 psi
@Temperature 100 °C,
Time 252000 sec
EO34, IRM 903 Oil; ASTM D471
 <= 1875 psi
@Temperature 100 °C,
Time 252000 sec
EO14, IRM 901 Oil; ASTM D471
 <= 1875 psi
@Temperature 23.0 °C,
Time 252000 sec
EF11 Fluid Resistance, Fuel A; ASTM D471
 <= 2000 psi
@Temperature 100 °C,
Time 252000 sec
A14 – Heat Resistance; ASTM D573
 1750 - 3250 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged; ASTM D573
Elongation at Break 350 %Original; ASTM D412
 <= 140 %
@Temperature 23.0 °C,
Time 252000 sec
EF21 Fluid Resistance, Fuel b; ASTM D471
 <= 175 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged; ASTM D573
 <= 192.5 %
@Temperature 100 °C,
Time 252000 sec
EO14, IRM 901 Oil; ASTM D471
 <= 192.5 %
@Temperature 100 °C,
Time 252000 sec
EO34, IRM 903 Oil; ASTM D471
 <= 210 %
@Temperature 100 °C,
Time 252000 sec
A14 – Heat Resistance; ASTM D573
 <= 262.5 %
@Temperature 23.0 °C,
Time 252000 sec
EF11 Fluid Resistance, Fuel A; ASTM D471
Compression Set <= 25 %
@Temperature 100 °C,
Time 79200 sec
B14; ASTM D395 Method B
 <= 25 %
@Temperature 100 °C,
Time 79200 sec
B34; ASTM D395 Method B
 <= 50 %
@Temperature 100 °C,
Time 79200 sec
ASTM D395 S
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 212 °F
Minimum Service Temperature, Air -20.0 °F
 
Descriptive Properties
Hardness20-50EF21 Fluid Resistance, Fuel B, 70 h @ 23°C, ASTM D471
 40-60EA14 – Water Resistance, Test Method D471, 70 h @ 100°C
 40-60EF11 Fluid Resistance, ASTM D471, Fuel A , 70 h @ 23°C
 45-60EO14, IRM 901 Oil, 70 h @ 100°C, ASTM D471
 45-60EO34, IRM 903 Oil, 70 h @ 100°C, ASTM D471
 45-75Heat Aged, ASTM D573, 70 h @ 100°C
 45-75A14 – Heat Resistance, ASTM D573, 70 hours @ 100°C
 55-65ASTM D2240
Oil Immersion<40% Volume ChangeASTM D471, IRM 903 Oil, 70 h @ 100°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBRPM027 / 315688

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.