MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Borealis Fibremod™ GD301FE Polypropylene, Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 30% Glass Fiber Filler

Material Notes: GD301FE is a 30% chemically coupled high performance glass fiber reinforced polypropylene compound intended for injection molding. This material shows excellent mechanical properties also at elevated temperatures. The product is available in standard black 9502. Applications: front end carriers, door module carriers, fans and shrouds, pump housings, pedal carriers, and air bag housings.

Former trade name for this product was Xmod™.

Information provided by Borealis AG

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.14 g/ccISO 1183
Linear Mold Shrinkage 0.0095 cm/cmBorealis Method
Melt Flow 4.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 106 MPaISO 527-2
Elongation at Break 3.2 %50mm/min; ISO 527-2
Tensile Modulus 7500 MPa1mm/min; ISO 527-2
Flexural Strength 145 MPaISO 178
Flexural Modulus 6500 MPa2mm/min; ISO 178
Charpy Impact Unnotched 54.0 kJ/m²
@Temperature -20.0 °C
ISO 179/1eU
 59.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 10.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 11.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 148 °CISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 158 °CISO 75-2
Vicat Softening Point 139 °C
@Load 5.10 kg
ISO 306
 
Processing PropertiesOriginal ValueComments
Feed Temperature 40.0 - 80.0 °C
Melt Temperature 230 - 280 °Cmass temperature
Mold Temperature 30.0 - 50.0 °C
Injection Velocity 100 - 200 mm/secFlow Front Speed
Hold Pressure 3.00 - 6.00 MPa
 
Descriptive Properties
Back Pressureas low as possible
Emission (µgC/g)< 50VDA 277
Fogging (mg)< 2DIN 75201
Screw Speedlow to medium

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Adell ER-16 Homopolymer Polypropylene, 30% Glass Reinforced
Borealis Fibremod™ GB205U Polypropylene Compound, Glass Fiber Reinforced
Borealis Fibremod™ GB306SAF Polypropylene, Glass Fiber Reinforced
Borealis Fibremod™ GB364WG Polypropylene Compound, Glass Fiber Reinforced
Borealis Fibremod™ GB366WG Polypropylene Compound, Glass Fiber Reinforced

PBOREA610 / 108869

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.