Physical Properties | Original Value | Comments |
---|
Density | 2.79 g/cc |
|
Chemical Properties | Original Value | Comments |
---|
Acid Class, SR | 1.0 |
Alkali Class, AR | 1.0 |
Stain Resistance Class, FR | 0.00 |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 560 |
Modulus of Elasticity | 82.0 GPa |
Poissons Ratio | 0.226 |
Shear Modulus | 33.4 GPa |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 7.20 µm/m-°C @Temperature -30.0 - 70.0 °C |
| 8.20 µm/m-°C @Temperature 20.0 - 300 °C |
Specific Heat Capacity | 0.760 J/g-°C |
Thermal Conductivity | 1.04 W/m-K |
Transformation Temperature, Tg | 583 °C |
Softening Point | 714 °C |
Annealing Point | 573 °C |
|
Optical Properties | Original Value | Comments |
---|
Refractive Index | 1.549 @Wavelength 2325.4 nm |
| 1.555 @Wavelength 1970.1 nm |
| 1.561 @Wavelength 1529.6 nm |
| 1.568 @Wavelength 1060 nm |
| 1.572 @Wavelength 852.1 nm |
| 1.576 @Wavelength 706.5 nm |
| 1.578 @Wavelength 656.3 nm |
| 1.579 @Wavelength 643.8 nm |
| 1.58 @Wavelength 632.8 nm |
| 1.582 @Wavelength 589.3 nm |
| 1.582 @Wavelength 587.6 nm |
| 1.585 @Wavelength 546.1 nm |
| 1.591 @Wavelength 486.1 nm |
| 1.592 @Wavelength 480 nm |
| 1.596 @Wavelength 1014 nm |
| 1.598 @Wavelength 435.8 nm |
| 1.604 @Wavelength 404.7 nm |
Abbe Number | 46.35 |
| 46.64 |
Optical Dispersion | 0.012495 |
| 0.012637 |
Transmission, Visible | 95.2 % @Thickness 25.0 mm, Wavelength 420 nm |
| 96.5 % @Thickness 25.0 mm, Wavelength 436 nm |
| 97.5 % @Thickness 25.0 mm, Wavelength 460 nm |
| 98.1 % @Thickness 10.0 mm, Wavelength 420 nm |
| 98.5 % @Thickness 25.0 mm, Wavelength 500 nm |
| 98.6 % @Thickness 10.0 mm, Wavelength 436 nm |
| 99 % @Thickness 10.0 mm, Wavelength 460 nm |
| 99.1 % @Thickness 25.0 mm, Wavelength 456 nm |
| 99.1 % @Thickness 25.0 mm, Wavelength 620 nm |
| 99.2 % @Thickness 25.0 mm, Wavelength 660 nm |
| 99.3 % @Thickness 25.0 mm, Wavelength 580 nm |
| 99.4 % @Thickness 25.0 mm, Wavelength 700 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 500 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 456 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 620 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 660 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 580 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 700 nm |
IR Transmittance | 46 % @Thickness 25.0 mm, Wavelength 2500 nm |
| 66 % @Thickness 25.0 mm, Wavelength 2325 nm |
| 73.3 % @Thickness 10.0 mm, Wavelength 2500 nm |
| 84.7 % @Thickness 10.0 mm, Wavelength 2325 nm |
| 89 % @Thickness 25.0 mm, Wavelength 1970 nm |
| 95.4 % @Thickness 10.0 mm, Wavelength 1970 nm |
| 98 % @Thickness 25.0 mm, Wavelength 1530 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 1530 nm |
| 99.3 % @Thickness 25.0 mm, Wavelength 1060 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 1060 nm |
UV Transmittance | 6.3 % @Thickness 10.0 mm, Wavelength 350 nm |
| 24 % @Thickness 25.0 mm, Wavelength 365 nm |
| 40 % @Thickness 25.0 mm, Wavelength 370 nm |
| 56.5 % @Thickness 10.0 mm, Wavelength 365 nm |
| 67 % @Thickness 25.0 mm, Wavelength 380 nm |
| 69.3 % @Thickness 10.0 mm, Wavelength 370 nm |
| 82 % @Thickness 25.0 mm, Wavelength 390 nm |
| 85.2 % @Thickness 10.0 mm, Wavelength 380 nm |
| 90 % @Thickness 25.0 mm, Wavelength 400 nm |
| 92 % @Thickness 25.0 mm, Wavelength 405 nm |
| 92.4 % @Thickness 10.0 mm, Wavelength 390 nm |
| 95.9 % @Thickness 10.0 mm, Wavelength 400 nm |
| 96.7 % @Thickness 10.0 mm, Wavelength 405 nm |
|
Descriptive Properties |
---|
Climatic resistance | 1 |
Grindability | 2 |
Phosphate resistance | 1 |
Stress optical coefficient | 2.73 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.