MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Akro-Plastic Akromid® B3 GF 40 1 L black (4581) PA6 + PP Dry, 40% Glass Filled, Heat Stabilized
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Polypropylene (PP)

Material Notes: Description: AKROMID B3 GF 40 1 L black (4581) is 40% glass fiber reinforced and heat stabilized polyamide-blend with a reduced density compared to standard PA6 GF 40. Applications are mainly technical components in the automotive and electronic industry, where a weight and cost reduction is required

Additive: Heat Stabilizer

Features:

  • Heat Stabilized
  • Low Density
Uses:
  • Automotive Applications
  • Electrical/Electronic Applications
  • Engineering Parts

Information provided by Akro-Plastic GmbH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.36 g/ccISO 1183
Filler Content 40 %ISO 1172
Moisture Absorption 1.2 %
@Temperature 70.0 °C
Humidity, 62% RH; ISO 1110
Linear Mold Shrinkage, Flow 0.0040 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cmISO 294-4
Melt Flow 7.0 g/10 min
@Load 5.00 kg,
Temperature 275 °C
ISO 1133
Spiral Flow 65.0 cmCross section: 7 mm x 3.5 mm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 160 MPa5 [mm/min]; ISO 527-2
Elongation at Break 3.2 %5 [mm/min]; ISO 527-2
Tensile Modulus 11000 MPa1 [mm/min]; ISO 527-2
Charpy Impact Unnotched 55.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 70.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 15.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 16.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 220 °CDIN EN 11357-1
Deflection Temperature at 1.8 MPa (264 psi) 200 °CUnannealed; ISO 75/A
Flammability, UL94 HB
@Thickness 0.800 mm
 
Processing PropertiesOriginal ValueComments
Feed Temperature 60.0 - 80.0 °C
Nozzle Temperature 270 - 290 °C
Zone 1 230 - 295 °C
Zone 2 230 - 295 °C
Zone 3 230 - 295 °C
Zone 4 230 - 295 °C
Melt Temperature 270 - 295 °C
Mold Temperature 70.0 - 100 °C
Drying Temperature 80.0 °C
Dry Time <= 2.00 hour
Hold Pressure 30.0 - 80.0 MPa
Back Pressure 5.00 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® KR 4350 PA6/6T (Dry)
Mitsubishi Chemical Advanced Materials Nylatron® MD PA6, Metal-detectable Nylon (ASTM Product Data Sheet)
Akro-Plastic Akromid® A3 GF 25 1 L black (4672) PA66 + PP, Dry, 25% Glass Filled
Akro-Plastic Akromid® B3 GF 40 9 RM-M natural (3414) PA6 + X, Dry, 40% Glass Filled
Bisalloy Steels BisPlate 80 Thickness 5 -<16 mm

PAKRO374 / 182961

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.