MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Total PS CPDS 856S Chlorine and Bromine Free Flame Retardant High Impact Polystyrene
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Flame Retardant

Material Notes: Total Petrochemicals Polystyrene 856S is a chlorine and bromine free flame retardant high impact polystyrene with excellent thermal stability and processability for injection molding.

Suitable Applications for Total Petrochemicals Polystyrene 850S include TV covers, Decoders, Hi-Fi and Internal parts for office equipment.

Information provided by Total Petrochemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.07 g/ccASTM D792
Water Absorption 0.070 %ASTM D570
Linear Mold Shrinkage 0.0040 cm/cmASTM D955
Melt Flow 3.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ASTM D1238
Spiral Flow 35.0 cm
@Temperature 220 °C
ASTM D3123
 52.0 cm
@Temperature 260 °C
ASTM D3123
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 97ASTM D785
Tensile Strength at Break 36.0 MPaASTM D638
Tensile Strength, Yield 35.0 MPaASTM D638
Elongation at Break 50 %ASTM D638
Tensile Modulus 2300 MPaASTM D638
Flexural Modulus 2300 MPaASTM D790
Izod Impact, Notched (ISO) 6.50 kJ/m²ASTM D256
 
Electrical PropertiesOriginal ValueComments
Surface Resistance >= 1.00e+13 ohmISO IEC 93
Dielectric Strength 160 kV/mmASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 91.0 µm/m-°CASTM D696
Vicat Softening Point 96.0 °C
@Load 1.02 kg
50°C per hour; ASTM D1525
Heat Distortion Temperature >= 180 °FASTM D648
Flammability, UL94 V-0
@Thickness 3.00 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Total PS CPDS 856 Flame Retardant Polystyrene
Celanese Zytel® FR7025V0F NC010 PA66-FR(30)
Advanced Elastomer Systems Santoprene® 101-64 W175 Thermoplastic Rubber

PTOTAL911 / 130636

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.