MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ATI Wah Chang Zircadyne® Alloy Zr 702
Categories: Metal; Nonferrous Metal; Zirconium Alloy

Material Notes: Zircadyne 702 is commercially pure zirconium. Alloy exhibits good ductility even at cryogenic temperatures and good strength comparable with other common engineering alloys.

Information provided by ATI Wah Chang

Key Words: UNS R60702
Vendors: Eagle Alloys Corporation is a leading supplier of quality metals and alloys. Our staff prides itself on working fast, efficiently and courteously to get you the information you need. Call (800) 237-9012 or visit www.EagleAlloys.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.235 lb/in³
Vapor Pressure 900 torr
@Temperature 3600 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 22700 psi
@Temperature 371 °C
 28700 psi
@Temperature 316 °C
 29100 psi
@Temperature 260 °C
 33300 psi
@Temperature 204 °C
 44200 psi
@Temperature 149 °C
 52800 psi
@Temperature 93.0 °C
 67900 psi
@Temperature 23.0 °C
Tensile Strength, Yield 11900 psi
@Temperature 371 °C
 14100 psi
@Temperature 316 °C
 18700 psi
@Temperature 260 °C
 20200 psi
@Temperature 204 °C
 28400 psi
@Temperature 149 °C
 38800 psi
@Temperature 93.0 °C
 46600 psi
@Temperature 23.0 °C
Elongation at Break 28.9 %
@Temperature 23.0 °C
 31.5 %
@Temperature 93.0 °C
 40.1 %
@Temperature 316 °C
 42.5 %
@Temperature 149 °C
 44.1 %
@Temperature 371 °C
 49 %
@Temperature 204 °C
 49 %
@Temperature 260 °C
Modulus of Elasticity 64.1 GPa
@Temperature 371 °C
 69.6 GPa
@Temperature 316 °C
 75.2 GPa
@Temperature 260 °C
 80.7 GPa
@Temperature 204 °C
 86.9 GPa
@Temperature 149 °C
 93.1 GPa
@Temperature 93.0 °C
 98.6 GPa
@Temperature 38.0 °C
 99.2 GPa
@Temperature 23.0 °C
Poissons Ratio 0.35
Shear Modulus 5250 ksi
@Temperature 23.0 °C
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 252.7 J/gLatent
Heat of Vaporization 1550 cal/gLatent
CTE, linear 3.50 µin/in-°F
@Temperature 149 °C
 3.90 µin/in-°F
@Temperature 260 °C
 4.10 µin/in-°F
@Temperature 371 °C
Melting Point 1852 °C
 
Component Elements PropertiesOriginal ValueComments
Fe + Cr <= 0.20 %
Hafnium, Hf <= 4.5 %
Zirconium, Zr >= 94.7 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sandvik Zr 702 Zirconium
ATI Wah Chang Zircadyne® Alloy Zr 705
Grade 702 Zirconium, Commercially Pure
Aluminum 6061-O
Industeel URANUS® 47N+ 25 Cr Super Duplex Stainless Steel with PREN = 40

NATIWC18 / 15073

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.