MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EMS-Grivory Grilon® BS 23 PA6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6)

Material Notes:

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.14 g/ccDry; ISO 1183
Water Absorption 9.0 %Sim. to ISO 62
Moisture Absorption 3.00 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0080 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.011 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 70.0 MPaDry; ISO 527-1/-2
Elongation at Break 8.0 %Dry; ISO 527-1/-2
 >= 50 %Conditioned; ISO 527-1/-2
Tensile Modulus 1300 MPaConditioned; ISO 527-1/-2
 3500 MPaDry; ISO 527-1/-2
Charpy Impact Unnotched 45.0 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
Dry; ISO 179/1eU
Charpy Impact, Notched 3.00 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eA
 4.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eA
 4.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eA
 20.0 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+10 ohm-cmConditioned; IEC 60093
 1.00e+12 ohm-cmDry; IEC 60093
Surface Resistance 1.00e+11 ohmIEC 60093
Dielectric Strength 22.0 kV/mmConditioned; IEC 60243-1
 24.0 kV/mmDry; IEC 60243-1
Comparative Tracking Index 600 VConditioned; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 70.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°CISO 11359-1/-2
Melting Point 222 °C10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 70.0 - 90.0 °CLong Term; ISO 2578
 180 °CShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 185 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °CISO 75-1/-2
Flammability, UL94 HBIEC 60695-11-10
 
Descriptive Properties
AutomotiveAir intake systems
 Interior
 Powertrain and Chassis
Electricals & ElectronicsElectrical appliances
FormGranules
Industry & Consumer goodsHousewares
 Mechanical Engineering
 Sports & Leisure
ProcessingInjection Molding
Product AttributesImproved flowability and demolding
 Nucleated

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® 8202C HS BK-102 PA6 (Dry)
INEOS Styrolution Terluran® HI-10 ABS
Global EPP PET SL PET + Solid Lubricant
GEHR Plastics PVC-U Polyvinylchloride
Envalior Akulon® K222-KGV5

PGRH215 / 156924

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.