MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Toyobo Celanex® 2008FC PBT
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: Product Description: Low molecular weight PBT for use in melt blown food contact applications. Celanex 200FC is a general purpose, unreinforced polybutylene terephthalate with a good balance of mechanical properties and processability for use in melt blown applications with food contact.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Forms: Pellets

Processing Method: Extrusion, Injection Molding

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.31 g/cc0.0473 lb/in³ISO 1183
Water Absorption 0.20 %0.20 %Equilibrium, 50% RH; ISO 62
Water Absorption at Saturation 0.45 %0.45 %ISO 62
Maximum Moisture Content 0.0200.020
Linear Mold Shrinkage, Flow 0.018 - 0.020 cm/cm0.018 - 0.020 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.018 - 0.020 cm/cm0.018 - 0.020 in/inISO 294-4
Melt Flow 275 g/10 min
@Load 2.16 kg,
Temperature 250 °C
275 g/10 min
@Load 4.76 lb,
Temperature 482 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7272ISO 2039-2
Tensile Strength at Break 60.0 MPa8700 psiISO 527-2/5
Elongation at Break 5.0 %5.0 %ISO 527-2/5
Tensile Modulus 2.60 GPa377 ksiISO 527-1
Flexural Strength 80.0 MPa11600 psiISO 178
Flexural Modulus 2.20 GPa319 ksiISO 178
Izod Impact, Notched (ISO) 3.15 kJ/m²1.50 ft-lb/in²ISO 180/1A
Charpy Impact Unnotched  3.78 J/cm²
@Temperature 22.8 °C
18.0 ft-lb/in²
@Temperature 73.0 °F
ISO 179/1eU
 4.41 J/cm²
@Temperature -30.0 °C
21.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  0.210 J/cm²
@Temperature -30.0 °C
1.00 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.273 J/cm²
@Temperature 22.8 °C
1.30 ft-lb/in²
@Temperature 73.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 62631-3-1
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 62631-3-2
Dielectric Constant  3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
IEC 60250
 3.3
@Frequency 100 Hz
3.3
@Frequency 100 Hz
IEC 60250
Dielectric Strength 15.0 kV/mm380 kV/inIEC 60243-1
Dissipation Factor 0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.0 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 101 µm/m-°C56.0 µin/in-°FISO 11359-2
Melting Point 225 °C437 °FISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 155 °C311 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 57.2 °C135 °FUnannealed; ISO 75-2/A
Glass Transition Temp, Tg 60.0 °C140 °FISO 11357-2
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 50.0 °C68.0 - 122 °FHopper
 250 - 260 °C482 - 500 °FHot Runner
Feed Temperature 230 - 240 °C446 - 464 °FInjection
Rear Barrel Temperature 230 - 240 °C446 - 464 °F
Middle Barrel Temperature 235 - 250 °C455 - 482 °F
Front Barrel Temperature 235 - 250 °C455 - 482 °F
Nozzle Temperature 250 - 260 °C482 - 500 °F
Zone 4 240 - 260 °C464 - 500 °FInjection
Melt Temperature 235 - 260 °C455 - 500 °F
Mold Temperature 65.0 - 92.8 °C149 - 199 °F
Drying Temperature 120 - 130 °C248 - 266 °F
Dry Time 4.00 hour4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCQ6172 / 310865

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.