MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Avient Bergamid™ A700 TM-YF Polyamide 66 (Nylon 66), Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes:

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.08 g/cc±0.02 g/cm³; DIN 53479
Moisture Absorption 2.2 %23C/50RH; ISO 62
Water Absorption at Saturation 6.7 %ISO 62
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 50.0 MPa
@Temperature 23.0 °C
dry as molded; ISO 527-2/50
Elongation at Yield 6.0 %
@Temperature 23.0 °C
dry as molded; ISO 527-2/50
Tensile Modulus 2000 MPa
@Temperature 23.0 °C
dry as molded; ISO 527-2/1
Charpy Impact Unnotched NB
@Temperature 23.0 °C
ISO 179/1eU
 NB
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 25.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Constant 3.3
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 90.0 kV/mmIEC 60243-1
Dissipation Factor 0.016
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesOriginal ValueComments
Melting Point 261 °CISO 3146
Maximum Service Temperature, Air 80.0 °CContinuous (GTP 50% Tensile); IEC 60216
 180 °CShort Time; IEC 60216
Deflection Temperature at 0.46 MPa (66 psi) 200 °CUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °CUnannealed; ISO 75-2/A
Flammability, UL94 HB
@Thickness 0.800 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Melt Temperature 270 - 290 °C
Mold Temperature 40.0 - 80.0 °C
Drying Temperature 80.0 °C
Dry Time 4.00 - 8.00 hourDesiccant Dryer
Back Pressure 50.0 - 150 MPa
 
Descriptive Properties
FormsPellets
Generic MaterialNylon 66
Generic NamePolyamide 66 (Nylon 66)
Processing MethodExtrusion
 Injection Molding
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
RoHS ComplianceRoHS Compliant
UL File NumberE76261Global

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Avient Bergamid™ A70 G30 U Polyamide 66 (Nylon 66)
Avient Edgetek® NN-25GB/000 Nylon 66 - 25% Glass Bead Reinforced
Nanocyl PLASTICYL™ PA1501 Polyamide 66 - Carbon Nanotube Masterbatch
Envalior Akulon® S223-G6 Nylon 66-30% Glass Reinforced (European and Asian Grade) (Cond)
Envalior Akulon® K240-HPG3 Impact Modified Nylon 6-15% Glass Reinforced (European Grade) (Dry)

PH0POL1457 / 146026

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.