MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPE RV-2670D Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink RV-2670D is a high performance thermoplastic elastomer, available in NAT and BLK, used in a variety of transportation applications. Sarlink RV-2670D is a high hardness, high density, filled grade with a 400k psi modulus that is UV stabilized and suitable for extrusion and injection molding.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Filled; Good Adhesion; Good Toughness; High Density; High Hardness; High Specific Gravity; Low Flow; Lubricated; Sunlight Resistant; Slip; UV Resistant; Weather Resistant

Uses: Automotive Applications; Automotive Exterior Parts; Automotive Exterior Trim; Racks

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion; Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.18 g/ccISO 1183
Viscosity 613 cP
@Shear Rate 206 1/s,
Temperature 200 °C
ASTM D3835
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 68
@Time 15.0 sec
Injection Molded; ISO 868
 69
@Time 5.00 sec
Injection Molded; ISO 868
 70
@Time 1.00 sec
Injection Molded; ISO 868
 69.3
@Treatment Temp. 125 °C,
Time 15.0 sec
Change in Air, 168 hr; ISO 888
 69.4
@Treatment Temp. 110 °C,
Time 15.0 sec
Change in Air, 1008 hr; ISO 888
 70.1
@Treatment Temp. 125 °C,
Time 1.00 sec
Change in Air, 168 hr; ISO 888
 70.1
@Treatment Temp. 125 °C,
Time 5.00 sec
Change in Air, 168 hr; ISO 888
 70.2
@Treatment Temp. 110 °C,
Time 5.00 sec
Change in Air, 1008 hr; ISO 888
 70.6
@Treatment Temp. 110 °C,
Time 1.00 sec
Change in Air, 1008 hr; ISO 888
Tensile Strength at Break 2590 psiAcross Flow, Type 1, 20 in/min; ISO 37
 3160 psiFlow, Type 1, 20 in/min; ISO 37
 2690 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
 2750 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
 3410 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
 3510 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
Tensile Stress at Strain 1850 psi
@Strain 100 %
Across Flow, Type 1, 20 in/min; ISO 37
 2500 psi
@Strain 100 %
Flow, Type 1, 20 in/min; ISO 37
 2150 psi
@Strain 100 %,
Treatment Temp. 110 °C
Across Flow, Type 1, Change in Air, 1008 hr; ISO 188
 2220 psi
@Strain 100 %,
Treatment Temp. 125 °C
Across Flow, Type 1, Change in Air, 6.61 in; ISO 188
 3230 psi
@Strain 100 %,
Treatment Temp. 110 °C
Flow, Type 1, Change in Air, 1008 hr; ISO 188
 3330 psi
@Strain 100 %,
Treatment Temp. 125 °C
Flow, Type 1, Change in Air, 168 hr; ISO 188
Elongation at Break 120 %Across Flow, Type 1, 20 in/min; ISO 37
 140 %Flow, Type 1, 20 in/min; ISO 37
 82.8 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
 115 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
 139 %
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
 153 %
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
Flexural Modulus 390000 psiASTM D790
Tear Strength 710 pliFlow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
 1000 pliAcross Flow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
Compression Set 67 %
@Temperature 22.8 °C,
Time 79200 sec
Type 1; ISO 815
 93 %
@Temperature 90.0 °C,
Time 252000 sec
Type 1; ISO 815
 94 %
@Temperature 70.0 °C,
Time 79200 sec
Type 1; ISO 815
 
Processing PropertiesOriginal ValueComments
Processing Temperature 380 - 450 °FInjection, Melt
Rear Barrel Temperature 380 - 450 °FInjection
Middle Barrel Temperature 380 - 450 °FInjection
Front Barrel Temperature 380 - 450 °FInjection
Nozzle Temperature 380 - 450 °FInjection
Zone 1 380 - 430 °FExtrusion
Zone 2 380 - 430 °FExtrusion
Zone 3 380 - 430 °FExtrusion
Zone 4 380 - 430 °FExtrusion
Zone 5 380 - 430 °FExtrusion
Die Temperature 380 - 430 °FExtrusion
Mold Temperature 60.0 - 110 °FInjection
Injection Pressure 200 - 1000 psiInjection
Back Pressure 25.0 - 50.0 psiInjection
Cushion 0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpmExtrusion
 50 - 100 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ1128 / 237619

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.