MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Lehvoss LUVOCOM® 16-8960/ES Polyarylamide with carbon fiber and steel fiber  (discontinued **)
Categories: Polymer; Thermoplastic; Polyarylamide (PAA)

Material Notes: Properties/attributes include: Electrically conductive, suitable for continuous discharging of statically-generated electricity (EMI-shielding). Strong, stiff parts. Low water absorption. Low influence from moisture and temperature to measures and electrical properties

Automotive industry, textile- and office machinery, apparatus- and precision engineering. Typical uses include: Handles, levers, rollers, body parts.

Processing: During processing the moisture level should not exceed 0.1%, otherwise molecular degradation and surface defects (e.g. smearing) may occur. Excessively high predrying temperatures may cause discoloration. The processing notes provided merely represent a recommendation for general use. Due to the large variety of machines, geometries and volumes of parts, etc., it may be necessary to employ different settings according to the specific application.

Information provided by Lehmann & Voss & Co.KG

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.41 g/ccISO 1183
Moisture Absorption <= 0.300 %
@Temperature 23.0 °C,
Time 86400 sec
Linear Mold Shrinkage 0.0020 - 0.0060 cm/cmDIN 16901
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 125 MPaISO 527-2
Elongation at Break 1.6 %ISO 527-2
Modulus of Elasticity 10.0 GPaISO 527-2
Flexural Strength 180 MPaISO 178
Flexural Modulus 9.00 GPaISO 178
Flexural Strain at Break 2.1 %Flexural Elongation @ Fmax; ISO 178
Charpy Impact Unnotched 19.0 kJ/m²
@Temperature -30.0 °C
ISO 179
 20.0 kJ/m²
@Temperature 23.0 °C
ISO 179 1eU
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity <= 10.0 ohm-cmIEC 60167
Surface Resistance <= 100 ohmIEC 60093
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 120 °CContinuous; UL 746B
 160 °CShort Term
Deflection Temperature at 1.8 MPa (264 psi) 230 °CISO 75-2/A
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 250 - 290 °C
Zone 1 260 - 300 °C
Zone 2 260 - 300 °C
Zone 3 260 - 300 °C
Melt Temperature 285 °C
Mold Temperature 110 - 140 °C
Drying Temperature 100 °C
@Time 21600 - 28800 sec
Dehumidifying dryer
 130 °C
@Time 14400 - 21600 sec
Vacuum Dryer
Moisture Content <= 0.10 %
 
Descriptive Properties
Colorblack

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lehvoss LUVOCOM® 1850-8023 PBT with carbon fiber
Lehvoss LUVOCOM® 1-8864/ES Polyamide 66 with steel fiber
Lehvoss LUVOCOM® 80-8003-3 Polyacetal-copolymer with carbon fiber
RTP Company EMI 660.5 Acrylonitrile Butadiene Styrene (ABS), Stainless Steel Fiber - Electrically Conductive - EMI/RFI/ESD Protection
RTP Company RTP 1399X67317C Polyphenylene Sulfide (PPS), GF, Stainless Steel Fiber, EMI

PLUU8883 / 193842

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.