System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Marco Polo MARPOL HDM 506 HDPE
Categories:
Polymer
;
Thermoplastic
;
Polyethylene (PE)
;
High Density (HDPE)
Material Notes:
Recommended Applications: Industrial caps and closures, industrial pails, packaging drum lids, recreational vehicle components.
Information provided by Marco Polo International, LLC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
0.945
g/cc
0.0341
lb/in³
ASTM D4883
ESCR 10% Igepal®
90
hour
90
hour
F50; ASTM D1693B
Melt Flow
4.0
g/10 min
@Load 2.16 kg,
Temperature 190 °C
4.0
g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Tensile Strength, Yield
23.4
MPa
3400
psi
ASTM D638
Elongation at Break
1000 %
1000 %
ASTM D638
Flexural Modulus, 1% Secant
1070
MPa
155000
psi
ASTM D790B
Izod Impact, Notched
0.961
J/cm
@Temperature -40.0 °C
1.80
ft-lb/in
@Temperature -40.0 °F
ASTM D256
Thermal Properties
Metric
English
Comments
Deflection Temperature at 0.46 MPa (66 psi)
71.1
°C
160
°F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
37.3
°C
99.1
°F
ASTM D648
Vicat Softening Point
121
°C
250
°F
Brittleness Temperature
<=
-75.0
°C
<=
-103
°F
ASTM D746
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PMARCO179 / 283776
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.