System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Fujipoly Industries Sarcon® 30Q Thin-Film QR
Categories:
Polymer
;
Film
;
Thermoset
;
Silicone
Material Notes:
Sarcon QR is Fujipolys originally developed High Heat Conductive/Low Hardness Silicone Rubber. Fine, high heat conductive ceramic particles are mixed with insulative silicone rubber.
Information provided by Fujipoly Industries
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Mechanical Properties
Original Value
Comments
Hardness, Shore A
55
ASTM D2240
63
60°C for 500 hrs with 95% RH; ASTM D2240
73
150°C for 1,000 hrs; ASTM D2240
80
200°C for 1,000 hrs; ASTM D2240
Tensile Strength, Yield
2.66
MPa
4.33
MPa
60°C for 500 hrs with 95% RH
5.33
MPa
150°C for 1,000 hrs
6.00
MPa
200°C for 1,000 hrs
Elongation at Yield
70 %
200°C for 1,000 hrs
103 %
147 %
60°C for 500 hrs with 95% RH
250 %
Tear Strength
0.500
kN/m
Electrical Properties
Original Value
Comments
Volume Resistivity
2.80e+14
ohm-cm
60°C for 500 hrs with 95% RH
1.00e+15
ohm-cm
3.20e+15
ohm-cm
150°C for 1,000 hrs
7.50e+15
ohm-cm
200°C for 1,000 hrs
Dielectric Constant
3.87
@Frequency 1e+6 Hz
After 1000 hrs at 200°C
3.88
@Frequency 1000 Hz
After 1000 hrs at 200°C
3.91
@Frequency 50 Hz
After 1000 hrs at 200°C
3.99
@Frequency 1000 Hz
After 1000 hrs at 150°C
3.99
@Frequency 1e+6 Hz
After 1000 hrs at 150°C
4.02
@Frequency 50 Hz
After 1000 hrs at 150°C
4.1
@Frequency 1e+6 Hz
After 500 hrs at 60°C with 95% RH
4.11
@Frequency 1e+6 Hz
4.12
@Frequency 1000 Hz
4.13
@Frequency 1000 Hz
After 500 hrs at 60°C with 95% RH
4.15
@Frequency 50 Hz
4.2
@Frequency 50 Hz
After 500 hrs at 60°C with 95% RH
Dielectric Strength
7.00
kV/mm
AC 60 Hz
10.0
kV/mm
150°C for 1,000 hrs
11.0
kV/mm
200°C for 1,000 hrs
11.0
kV/mm
60°C for 500 hrs with 95% RH
Dielectric Breakdown
7000
V
Withstand Voltage [V/min]; AC 60 Hz
Dissipation Factor
0.0022
@Frequency 1e+6 Hz
After 1000 hrs at 150°C
0.0022
@Frequency 1e+6 Hz
After 1000 hrs at 200°C
0.0022
@Frequency 1e+6 Hz
0.0026
@Frequency 1000 Hz
After 1000 hrs at 150°C
0.0027
@Frequency 1e+6 Hz
After 500 hrs at 60°C with 95% RH
0.0031
@Frequency 1000 Hz
After 1000 hrs at 200°C
0.0035
@Frequency 50 Hz
After 1000 hrs at 200°C
0.0035
@Frequency 1000 Hz
0.0039
@Frequency 50 Hz
After 1000 hrs at 150°C
0.0064
@Frequency 50 Hz
0.0070
@Frequency 1000 Hz
After 500 hrs at 60°C with 95% RH
0.0132
@Frequency 50 Hz
After 500 hrs at 60°C with 95% RH
Thermal Properties
Original Value
Comments
Maximum Service Temperature, Air
182
°C
Minimum Service Temperature, Air
-60.0
°C
Flammability, UL94
V-0
Descriptive Properties
Color
Grey
Thermal Impedance
0.57°C/W
FTM P-3010; ASTM D5470
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
PFUJIP25 / 39158
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.