MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chromium Copper, UNS C18400, TF00 Temper flat products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent cold workability; good hot workability.

Applications: resistance welding electrodes, seam welding wheels, switch gear, electrode holder jaws, cable connectors, current carrying arms and shafts, circuit breaker parts, molds, spot welding tips, flash welding electrodes, electrical and thermal conductors requiring strength, switch contacts.

Test specimens: flat products - 1mm thickness aged 3 hours at 500°C.

UNS C18200, UNS C18400, and UNS C18500 have similar compositions and mechanical properties.

Key Words: CDA 184, CA184
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.89 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 59
Tensile Strength, Ultimate 350 MPa
Tensile Strength, Yield 250 MPa
Elongation at Break 22 %In 50 mm
Modulus of Elasticity 130 GPa
Poissons Ratio 0.30
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 80 %
Shear Modulus 50.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000216 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.6 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.385 J/g-°C
Thermal Conductivity 187 BTU-in/hr-ft²-°F
Melting Point 1070 - 1075 °C
Solidus 1070 °C
Liquidus 1075 °C
 
Processing PropertiesOriginal ValueComments
Solution Temperature 980 - 1000 °CFor 10-30 minutes, water quench
Aging Temperature 425 - 500 °CFor 2-4 hours
Hot-Working Temperature 800 - 925 °C
Precipitation Temperature 860 °F
@Time 180 sec
Air
 
Component Elements PropertiesOriginal ValueComments
Arsenic, As <= 0.0050 %
Calcium, Ca <= 0.0050 %
Chromium, Cr 0.40 - 1.2 %
Copper, Cu 99.2 %
Iron, Fe <= 0.15 %
Lithium, Li <= 0.050 %
Other, total <= 0.20 %
Phosphorus, P <= 0.050 %
Silicon, Si <= 0.10 %
Zinc, Zn <= 0.70 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chromium Copper, UNS C18400
Chromium Copper, UNS C18400, TB00 Temper flat products
Chromium Copper, UNS C18400, TD08 Temper 4 mm rod
Chromium Copper, UNS C18200, TH04 Temper TH04, Cold Worked 28% tube
Chromium Copper, UNS C18400 TH03 Temper (cold worked 6%) 13 mm rod

MC18400b3 / 10772

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.