MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

BASF Palatinol® 11P-E (DUP) Linear Phthalate
Categories: Other Engineering Material; Additive/Filler for Polymer

Material Notes: Formula: C30H50O4

Description: Palatinol® 11P-E plasticizer is a linear phthalate ester based on a predominately linear C11 alcohol. Palatinol 11P-E exhibits very low volatility and good processing characteristics with vinyl resin. Its viscosity is relatively low in relation to its molecular weight. Palatinol 11P-E is inhibited with 0.1% by weight of 1,1,3-tris(2-methyl-4-hydroxy 5-t butylphenyl) butane.

Applications: Vinyl resin compounders choose Palatinol 11P-E over DTDP for its lower viscosity, greater resin compatibility, faster dry blending and superior efficiency. When formulated to equal concentrations, Palatinol 11P-E provides equal electrical properties in 90°C and 105°C wire insulation compounds. With its lower viscosity, high thermal resistance, permanence and low volatility, Palatinol 11P-E is well suited for demanding applications such as automotive interior (instrument panel skins), building wire insulation, 90° THW and 105° THW, automotive wire harness and vinyl roofing membrane.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.948 - 0.955 g/cc0.0342 - 0.0345 lb/in³ASTM D4052
Solubility of Water 0.0015 %0.0015 %
Solubility in Water <= 1.0e-6 %<= 1.0e-6 %
Viscosity  27 cP
@Temperature 40.0 °C
27 cP
@Temperature 104 °F
Absolute
 71 cP
@Temperature 20.0 °C
71 cP
@Temperature 68.0 °F
Absolute
 255 cP
@Temperature 0.000 °C
255 cP
@Temperature 32.0 °F
Absolute
Molecular Weight 474 g/mol474 g/mol
Vapor Pressure <= 0.000800 bar<= 0.600 torr
 
Chemical PropertiesMetricEnglishComments
Total Acid Number <= 0.10<= 0.10[mg KOH/g]; ASTM D1045
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  76
@Time 15.0 sec
76
@Time 0.00417 hour
Plasticizer conc. in vinyl film 70 phr; ASTM D 2240
 88
@Time 15.0 sec
88
@Time 0.00417 hour
Plasticizer conc. in vinyl film 50 phr; ASTM D 2240
 93
@Time 15.0 sec
93
@Time 0.00417 hour
Plasticizer conc. in vinyl film 40 phr; ASTM D 2240
Tensile Strength 14.8 MPa2150 psiPlasticizer conc. in vinyl film 70 phr; ASTM D638
 18.5 MPa2680 psiPlasticizer conc. in vinyl film 50 phr; ASTM D638
 20.6 MPa2990 psiPlasticizer conc. in vinyl film 40 phr; ASTM D638
Elongation at Break 255 %255 %Plasticizer conc. in vinyl film 40 phr; ASTM D638
 285 %285 %Plasticizer conc. in vinyl film 50 phr; ASTM D638
 325 %325 %Plasticizer conc. in vinyl film 70 phr; ASTM D638
100% Modulus  7.93 MPa
@Strain 100 %
1150 psi
@Strain 100 %
Plasticizer conc. in vinyl film 70 phr; ASTM D638
 12.1 MPa
@Strain 100 %
1750 psi
@Strain 100 %
Plasticizer conc. in vinyl film 50 phr; ASTM D638
 16.5 MPa
@Strain 100 %
2390 psi
@Strain 100 %
Plasticizer conc. in vinyl film 40 phr; ASTM D638
Torsional Stiffness  310 MPa
@Temperature -15.0 °C
45000 psi
@Temperature 5.00 °F
Plasticizer conc. in vinyl film 40 phr; ASTM D1043
 310 MPa
@Temperature -30.0 °C
45000 psi
@Temperature -22.0 °F
Plasticizer conc. in vinyl film 50 phr; ASTM D1043
 310 MPa
@Temperature -45.0 °C
45000 psi
@Temperature -49.0 °F
Plasticizer conc. in vinyl film 70 phr; ASTM D1043
 
Thermal PropertiesMetricEnglishComments
CTE, linear 790 µm/m-°C439 µin/in-°F
Boiling Point 262 °C
@Pressure 1.32e+6 MPa
504 °F
@Pressure 1.91e+8 psi
Pour Point -9.00 °C15.8 °F
Brittleness Temperature -50.0 °C-58.0 °FPlasticizer conc. in vinyl film 70 phr; ASTM D746
 -42.0 °C-43.6 °FPlasticizer conc. in vinyl film 50 phr; ASTM D746
 -32.0 °C-25.6 °FPlasticizer conc. in vinyl film 40 phr; ASTM D746
Flash Point 254 °C489 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.4811.481
 
Processing PropertiesMetricEnglishComments
Moisture Content 0.10 %0.10 %ASTM E203
 
Descriptive Properties
Color<50APAH, ASTM D5386
CompositionEster content>99.6%, ASTM D3465

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASG0737 / 132370

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.