MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Hostacom HBG H02 BLACK Polypropylene with 20% Glass Fiber Filler
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 20% Glass Fiber Filler

Material Notes: Hostacom HBG H02 BLACK is a 20% glass fiber reinforced PP homopolymer, with very low melt flow rate, low creep under load at elevated temperatures, excellent hot water resistance and high dimensional stability. This grade is delivered in BLACK color version. Dry material before processing. Applications: Under hood

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ISO 1183-1A
Melt Flow 0.87 g/10 min
@Load 5.00 kg,
Temperature 230 °C
0.87 g/10 min
@Load 11.0 lb,
Temperature 446 °F
ISO 1133-1
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 65.0 MPa9430 psiISO 527-1,-2
Elongation at Yield 4.0 %4.0 %ISO 527-1,-2
Tensile Modulus 4.50 GPa653 ksiISO 527-1,-2
Charpy Impact Unnotched 4.50 J/cm²
@Temperature 23.0 °C
21.4 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1/1eU
Charpy Impact, Notched 1.20 J/cm²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 112 °C234 °Funannealed; ISO 75A-1,-2
Vicat Softening Point 120 °C248 °FB50; ISO 306
 
Descriptive Properties
Processing MethodInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEQT7966 / 219603

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.