MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Total XSene® HD55110 High Density Polyethylene - Blown Film
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Film Grade

Material Notes: HDPE HD55110 is a bimodal high density polyethylene with a particular molecular design developed with Total Petrochemicals Double Loop Technology™.

HDPE HD55110 has been especially designed for applications where high film properties can be obtained both in pure, in blend or in coextrusion films.

HDPE HD55110 can be used in high neck extrusion as well as low neck extrusion and is dedicated to several applications such as food packaging, lamination films, carrier bags, pouches, industrial packaging and hygiene packaging. Very thin films can also be easily achieved (down to 10 microns).

Information provided by Total Petrochemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.955 g/cc0.955 g/ccISO 1183
Thickness >= 10.0 microns>= 0.394 mil
 12.0 microns0.472 milfor samples tested on this data sheet
Melt Flow  0.30 g/10 min
@Load 5.00 kg,
Temperature 190 °C
0.30 g/10 min
@Load 11.0 lb,
Temperature 374 °F
ISO 1133
 11 g/10 min
@Load 21.6 kg,
Temperature 190 °C
11 g/10 min
@Load 47.6 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 39.0 MPa5660 psiISO 527-3
Film Tensile Strength at Yield, TD 30.0 MPa4350 psiISO 527-3
Film Elongation at Break, MD 308 %308 %ISO 527-3
Film Elongation at Break, TD 460 %460 %ISO 527-3
Elmendorf Tear Strength, MD 0.600 g/micron15.2 g/milISO 6383-2
Elmendorf Tear Strength, TD 4.60 g/micron117 g/milISO 6383-2
Dart Drop Test 170 g0.375 lbISO 7765-1
Film Tensile Strength at Break, MD 64.0 MPa9280 psiISO 527-3
Film Tensile Strength at Break, TD 54.0 MPa7830 psiISO 527-3
 
Thermal PropertiesMetricEnglishComments
Melting Point 132 °C270 °FISO 11357
Vicat Softening Point 130 °C266 °FISO 306
 
Processing PropertiesMetricEnglishComments
Processing Temperature 180 - 230 °C356 - 446 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
SIDPEC EGYPTENE® HD 5218 EA HDPE Injection Molding
Total 53090 High Density Polyethylene - Blow Molding
Total XSene® 55060 High Density Polyethylene - Blow Molding
Total Xsene® BM 593 HDPE, blow molding
Overview of materials for High Density Polyethylene (HDPE), Film Grade

PTOTAL724 / 130449

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.