MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Ensinger TECASINT™ 2011 Polyimide (PI)
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: TECASINT™ 2000 series of polyimide stock shapes provide a superior combination of high temperature and bearing and wear, properties that make it an ideal choice for the most demanding applications. TECASINT™ 2011 is very pure, and exhibits low outgassing. It is also characterized by it’s long term thermal stability, outstanding wear resistance, high creep resistance, and strength up to its continuous use temperature of 536° F. TECASINT™ 2021 contains 15% graphite and is also available for applications requiring improved wear resistance & lower coefficient of friction.
  • Superior high temperature characteristics (TECASINT™ 2000 series can operate up to 536° F continuously)
  • Excellent long-term thermal stability
  • Outstanding bearing and wear properties (at elevated temperatures, TECASINT™ 2000 formulations offer superior wear rates)
  • Excellent creep resistance
  • High strength and stiffness properties
  • High purity characteristics (only extremely low levels of extractables and ionic impurities are apparent in TECASINT™ 2011)
  • Good chemical resistance (TECASINT™ 2000 series is not attacked by common solvents or fuels and is acceptable for use in contact with many acids)

TECASINT™ 2000 series with their superior physical properties, are ideal for applications in the aerospace, nuclear, automotive, electrical/electronics, and chemical processing industries. TECASINT™ shapes are excellent candidates for high purity applications in the semiconductor processing industry. Typical components produced from TECASINT™ applications include seals, thrust washers, bushings and wear pads in transportation/off-highway equipment, insulating and support elements in electrical welding and brazing equipment, and wafer-handling components in the harsh environment of semiconductor plasma ovens. Pump and valve seals, vanes, and piston rings are also commonly produced from TECASINT™ series materials.

Information Provided by Ensinger Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.38 g/cc
@Temperature 23.0 °C
DIN 53 479
Water Absorption 0.47 %
@Temperature 23.0 °C,
Time 86400 sec
EN ISO 62
 1.65 %
@Temperature 80.0 °C,
Time 86400 sec
EN ISO 62
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 90
@Temperature 23.0 °C
DIN 53 505
Tensile Strength, Yield 118 MPa
@Temperature 23.0 °C
EN ISO 527
Elongation at Break 4.5 %
@Temperature 23.0 °C
EN ISO 527
Tensile Modulus 3700 MPa
@Temperature 23.0 °C
EN ISO 527
Flexural Strength 177 MPa
@Temperature 23.0 °C
EN ISO 178
Flexural Modulus 2150 MPa
@Temperature 300 °C
EN ISO 178
 2300 MPa
@Temperature 250 °C
EN ISO 178
 3600 MPa
@Temperature 23.0 °C
EN ISO 178
Flexural Strain at Yield 6.1 %EN ISO 178
Compressive Yield Strength 105 MPa10% Strain; EN ISO 604
Compressive Strength 486 MPa
@Temperature 23.0 °C
EN ISO 604
Compressive Modulus 1713 MPa
@Temperature 23.0 °C
EN ISO 604
Charpy Impact Unnotched 8.79 J/cm²EN ISO 179
Charpy Impact, Notched 0.930 J/cm²
@Temperature 23.0 °C
EN ISO 179
Compression Set 58 %Compression at Break; EN ISO 604
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cm
@Temperature 23.0 °C
IEC 60093
Surface Resistance 1.00e+15 ohm
@Temperature 23.0 °C
IEC 60093
Dielectric Constant 4.1
@Frequency 10000 Hz,
Temperature 23.0 °C
IEC 60250
 4.1
@Frequency 100000 Hz,
Temperature 23.0 °C
IEC 60250
 4.2
@Frequency 100 Hz,
Temperature 23.0 °C
IEC 60250
 4.2
@Frequency 1000 Hz,
Temperature 23.0 °C
IEC 60250
Dielectric Strength 21.8 kV/mm
@Temperature 23.0 °C
DC; ISO 60243-1
 
Thermal PropertiesOriginal ValueComments
CTE, linear 54.0 µm/m-°C
@Temperature 50.0 - 200 °C
DIN 53 752
 61.0 µm/m-°C
@Temperature 200 - 300 °C
DIN 53 752
Specific Heat Capacity 0.925 J/g-°C
Thermal Conductivity 0.220 W/m-K
@Temperature 40.0 °C
ISO 8302
Maximum Service Temperature, Air 300 °C
Deflection Temperature at 1.8 MPa (264 psi) 325 °CDIN 53 461
Glass Transition Temp, Tg 370 °CDMTA
Flammability, UL94 V-0
 
Descriptive Properties
ColorBrown
DIN-AbbreviationPI

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ensinger TECASINT 1011 Polyimide (PI)
Ensinger TECASINT 5011 Polyimide (PI)
Ensinger TECASINT 1101 Polyimide (PI)
Ensinger TECASINT™ 2021 Polyimide, 15% Graphite (PI)
Ensinger TECASINT™ 2021 Polyimide, Brown (PI)

PENSIN051 / 98112

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.