MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Zylog Neoplast® 187 FT EB Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Neoplast 187 FT EB is a hard, dynamically vulcanized thermoplastic vulcanizate (TPV), based on polyolefin chemistry, and is intended for Injection Molding, Blow Molding and Extrusion applications.

RoHS Compliant, UV Stabilized

Information provided by Zylog Plastalloys Pvt. Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.960 g/cc0.960 g/ccASTM D 792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9292ASTM D 2240
 93
@Time 605000 sec
93
@Time 168 hour
Heat Aging; ASTM D 2240/ASTM D 573
Tensile Strength, Ultimate 16.7 MPa2420 psi500 mm/min; ASTM D 412
 18.3 MPa
@Time 605000 sec
2660 psi
@Time 168 hour
Heat Aging; ASTM D 412/ASTM D 573
Elongation at Break 600 %600 %500 mm/min; ASTM D 412
 528 %
@Time 605000 sec
528 %
@Time 168 hour
Heat Aging; ASTM D 412/ASTM D 573
100% Modulus 10.8 MPa
@Strain 100 %
1560 psi
@Strain 100 %
500 mm/min; ASTM D 412
Tear Strength 49.0 kN/m280 pli500 mm/min; ASTM D 624
Compression Set 48 %
@Temperature 23.0 °C,
Time 79200 sec
48 %
@Temperature 73.4 °F,
Time 22.0 hour
ASTM B 395
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 135 °C275 °FContinuous; SAE J 2236
Brittleness Temperature -55.0 °C-67.0 °FASTM D 746

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Termopol Termoton® V2GA1065A TPV Compound
Celanese SO.F.TER Forprene® 6NE.A75 Extrusion Grade TPE
Celanese SO.F.TER Forprene® 6NE.A65 Extrusion Grade TPE
Barlog Plastics KEBAFLEX E D 50.1 TPE-V, Shore D50
Barlog Plastics KEBAFLEX E 65.1 TPE-V, Shore A65

PZYLOG951 / 157267

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.