MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
American Longleaf Pine Wood
Categories: Wood and Natural Products; Wood; Softwood

Material Notes: Softwood. Relatively easy to work with hand tools. Data is based on small, clear, air-dried samples unless specified.

Property values marked by an asterisk (*) have been taken from an unusually old reference source.

Key Words: Pinus palustris; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.550 g/ccOven Dry Weight/Unseasoned Volume
 41.0 lb/ft³Unseasoned*
 
Mechanical PropertiesOriginal ValueComments
Hardness, Wood Indentation 2400 NEnd. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 2600 NSide. Force required to imbed a 0.444 inch steel ball to one-half its diameter
Tensile Strength, Ultimate 290 psiPerpendicular to Grain*
Modulus of Rupture 0.101 GPaIn Bending
 8.70 ksiStatic Bending*
Flexural Yield Strength 64.1 MPaBending stress at proportional limit
 5400 psiFiber Stress at Elastic Limit; Static Bending*
Flexural Modulus 13.8 GPaIn Bending
 1630 ksiStatic Bending*
Compressive Strength 57.9 - 58.6 MPaParallel to Grain
 600 psiPerpendicular to Grain*
 2840 psiParallel to Grain*
 4390 psiMax Crushing Strength Parallel to Grain*
Poissons Ratio 0.332µLR, 12% Moisture Content
 0.342µTR, 12% Moisture Content
 0.365µLT, 12% Moisture Content
 0.384µRT, 12% Moisture Content
Shear Strength 10.3 MPaOrientation Unknown
 1070 psiParallel to Grain*
Impact 3.5in-lb/in³; Work to Elastic Limit; Unseasoned Sample; Impact Bending*
 10800psi; Fiber Stress at Elastic Limit; Unseasoned Sample; Impact Bending*
Work to Elastic Limit 1.00 in-lb/in³Static Bending*
Work to Maximum Load 8.00 in-lb/in³Static Bending*
Cleavage 32.0 kN/mTangential surface of failure, Unseasoned*
 33.0 kN/mRadial surface of failure, Unseasoned*
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.960 BTU-in/hr-ft²-°FOven Dry
 1.20 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 5.3 %Radial; Unseasoned to Oven Dry*
 7.5 %Tangential; Unseasoned to Oven Dry*
 12.4 %Volumetric; Unseasoned to Oven Dry*

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
American Eastern White Pine Wood
American Pine Wood
Southern Pine Wood
North American Loblolly Pine Wood
Northern White Pine Wood

PTSAI / 71292

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.