MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ovako 30MnVS6 EN10267:1998 Steel, +AR
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: 30MnVS6 is a micro alloyed cold heading steel which is used for example for short and longshaft ball points, threaded and heavy duty anchor bolts

Information provided by Ovako

Key Words: 9830 - 28MnV6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 700 - 900 MPa102000 - 131000 psiAll formats
Tensile Strength, Yield >= 450 MPa>= 65300 psiReh, All formats
Elongation at Break 14 %14 %All formats
Reduction of Area 30 %30 %All formats
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 370 °C698 °FMS
 720 °C1330 °FAC1
 800 °C1470 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.26 - 0.33 %0.26 - 0.33 %
Chromium, Cr <= 0.30 %<= 0.30 %
Iron, Fe 96.69 - 98.29 %96.69 - 98.29 %As Balance
Manganese, Mn 1.2 - 1.6 %1.2 - 1.6 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si 0.15 - 0.80 %0.15 - 0.80 %
Sulfur, S 0.020 - 0.060 %0.020 - 0.060 %
Vanadium, V 0.080 - 0.20 %0.080 - 0.20 %
 
Descriptive Properties
WeldabilityCEV 0.65max
 Pcm 0.43max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NOVAKO237 / 234536

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.