MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SYNTHOS Krasten® 336M High Impact Polystyrene
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Impact Modified

Material Notes: Easy flow grade. Processed by injection moulding of intricate and thin-walled products that enables high production output.

Synthos was formerly known as Kaucuk. All information provided by Synthos.

Key Words: HIPS
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.04 g/ccISO 1183
Linear Mold Shrinkage 0.0030 - 0.0060 cm/cmInternal; 50x50mm
Melt Flow 11 - 13 g/10 min
@Load 5.00 kg,
Temperature 200 °C
Granulate; ISO 1133/H
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 80.0 MPaFm=358N; Ø 50x4mm; ISO 2039-1
Tensile Strength at Break 24.0 MPa
@Temperature 23.0 °C
50mm/min; ISO 527-2/1A/50
Tensile Strength, Yield 28.0 MPa
@Temperature 23.0 °C
50mm/min; ISO 527-2/1A/50
Elongation at Break 35 %50mm/min; ISO 527-2/1A/50
Tensile Modulus 2300 MPa
@Temperature 23.0 °C
1mm/min; ISO 527-2/1A/1
Flexural Strength 42.0 MPa
@Temperature 23.0 °C
2mm/min; 80x10x4mm; ISO 178
Izod Impact, Notched (ISO) 6.00 kJ/m²
@Temperature 23.0 °C
80x10x4mm, r=0.25; V-notch; ISO 180/1A
Izod Impact, Unnotched (ISO) 55.0 kJ/m²
@Temperature 23.0 °C
80x10x4mm; ISO 180/1U
Charpy Impact Unnotched 5.00 J/cm²
@Temperature 23.0 °C
80x10x4mm; ISO 179/1fU
 7.00 J/cm²
@Temperature 23.0 °C
80x10x4mm; ISO 179/1eU
Charpy Impact, Notched 0.500 J/cm²
@Temperature 23.0 °C
80x10x4mm, r=0.25; V-notch; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+16 ohm-cm500V; Ø 93x3mm; IEC 93
Surface Resistance >= 5.00e+14 ohm500V; Ø 93x3mm; IEC 93
Dielectric Constant <= 3.0
@Frequency 50 Hz
500V; Ø 93x3mm; IEC 250
Dielectric Strength >= 28.0 kV/mmTransformer Oil; Ø 93x3mm; IEC 243-1
Dissipation Factor <= 0.0010
@Frequency 50 Hz
500V; Ø 93x3mm; IEC 250
Arc Resistance >= 70 secØ 93x3mm; IEC 61 621
Comparative Tracking Index >= 300 VSolution A; Ø 93x3mm; IEC 112
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C80x10x4mm; ISO 75-2/Af
Vicat Softening Point 82.0 °C50°C/h; 50N; 10x10x4mm; ISO 306/B50
 89.0 °C50°C/h; 10N; 10x10x4mm; ISO 306/A50
 93.0 °C120°C/h; 10N; 10x10x4mm; ISO 306/A120
Flammability, UL94 HB
@Thickness 1.60 mm
Tested in EZÚ Praha
 HB
@Thickness 3.00 mm
Tested in EZÚ Praha
Glow Wire Test 650 °CØ 93x3mm; IEC 695-2-1

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
SYNTHOS Krasten® 552M High Impact Polystyrene
IRPC Polimaxx Polene GP150 Polystyrene
I. Stern RT441M High Impact Polystyrene
Global GP-150 High Impact Polystyrene
FKuR Kunststoff Biograde® C 6530 Biodegradable Plastic Compound

PSYNT012 / 82625

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.