MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik 3R60 Seamless tube and pipe
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Sandvik 3R60 is an austenitic chromium-nickel steel with minimum 2.5% molybdenum and a low carbon content.

3R60 is also supplied in a variant for the urea industry, 3R60 Urea Grade. See data sheet S-1843-ENG.

Information provided by Sandvik

ASTM 316, 316L; UNS S31603, S31600; EN 1.4435, 1.4436

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.00 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B <= 90
Tensile Strength, Ultimate 515 - 690 MPa
 >= 380 MPa
@Temperature 400 °C
 >= 400 MPa
@Temperature 200 °C
 >= 450 MPa
@Temperature 100 °C
Tensile Strength, Yield >= 220 MPa
@Strain 0.2 %
 >= 250 MPa
@Strain 1 %
 >= 98.0 MPa
@Strain 0.2 %,
Temperature 400 °C
 >= 110 MPa
@Strain 0.2 %,
Temperature 600 °C
 >= 115 MPa
@Strain 0.2 %,
Temperature 550 °C
 >= 120 MPa
@Strain 0.2 %,
Temperature 450 °C
 >= 120 MPa
@Strain 0.2 %,
Temperature 500 °C
 >= 125 MPa
@Strain 0.2 %,
Temperature 400 °C
 >= 125 MPa
@Strain 1 %,
Temperature 400 °C
 >= 127 MPa
@Strain 0.2 %,
Temperature 200 °C
 >= 130 MPa
@Strain 0.2 %,
Temperature 350 °C
 >= 135 MPa
@Strain 1 %,
Temperature 600 °C
 >= 135 MPa
@Strain 0.2 %,
Temperature 300 °C
 >= 140 MPa
@Strain 1 %,
Temperature 550 °C
 >= 140 MPa
@Strain 0.2 %,
Temperature 250 °C
 >= 145 MPa
@Strain 1 %,
Temperature 450 °C
 >= 145 MPa
@Strain 1 %,
Temperature 500 °C
 >= 150 MPa
@Strain 1 %,
Temperature 400 °C
 >= 150 MPa
@Strain 0.2 %,
Temperature 200 °C
 >= 155 MPa
@Strain 1 %,
Temperature 350 °C
 >= 155 MPa
@Strain 0.2 %,
Temperature 100 °C
 >= 155 MPa
@Strain 1 %,
Temperature 300 °C
 >= 165 MPa
@Strain 0.2 %,
Temperature 150 °C
 >= 170 MPa
@Strain 1 %,
Temperature 300 °C
 >= 170 MPa
@Strain 1 %,
Temperature 250 °C
 >= 180 MPa
@Strain 1 %,
Temperature 200 °C
 >= 180 MPa
@Strain 0.2 %,
Temperature 100 °C
 >= 190 MPa
@Strain 1 %,
Temperature 100 °C
 >= 195 MPa
@Strain 1 %,
Temperature 150 °C
 >= 200 MPa
@Strain 0.2 %,
Temperature 50.0 °C
 >= 215 MPa
@Strain 1 %,
Temperature 100 °C
 >= 230 MPa
@Strain 1 %,
Temperature 50.0 °C
Elongation at Break >= 40 %
 >= 35 %
@Thickness 50.8 mm
Rupture Strength 18.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
 25.0 MPa
@Temperature 725 °C,
Time 3.60e+8 sec
 33.0 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
 37.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
 46.0 MPa
@Temperature 675 °C,
Time 3.60e+8 sec
 49.0 MPa
@Temperature 725 °C,
Time 3.60e+7 sec
 64.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
 64.0 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
 83.0 MPa
@Temperature 675 °C,
Time 3.60e+7 sec
 86.0 MPa
@Temperature 625 °C,
Time 3.60e+8 sec
 108 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
 108 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
 137 MPa
@Temperature 575 °C,
Time 3.60e+8 sec
 137 MPa
@Temperature 625 °C,
Time 3.60e+7 sec
 172 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
 177 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
 214 MPa
@Temperature 575 °C,
Time 3.60e+7 sec
 255 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
Modulus of Elasticity 200 GPa
 165 GPa
@Temperature 500 °C
 172 GPa
@Temperature 400 °C
 179 GPa
@Temperature 300 °C
 186 GPa
@Temperature 200 °C
 194 GPa
@Temperature 100 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.5 µm/m-°C
@Temperature 30.0 - 100 °C
 17.0 µm/m-°C
@Temperature 30.0 - 200 °C
 17.5 µm/m-°C
@Temperature 30.0 - 300 °C
 18.0 µm/m-°C
@Temperature 30.0 - 400 °C
 18.0 µm/m-°C
@Temperature 30.0 - 500 °C
 18.5 µm/m-°C
@Temperature 30.0 - 700 °C
 18.5 µm/m-°C
@Temperature 30.0 - 600 °C
Specific Heat Capacity 0.485 J/g-°C
@Temperature 20.0 °C
 0.500 J/g-°C
@Temperature 100 °C
 0.515 J/g-°C
@Temperature 200 °C
 0.525 J/g-°C
@Temperature 300 °C
 0.540 J/g-°C
@Temperature 400 °C
 0.555 J/g-°C
@Temperature 500 °C
 0.575 J/g-°C
@Temperature 600 °C
Thermal Conductivity 14.0 W/m-K
@Temperature 20.0 °C
 15.0 W/m-K
@Temperature 100 °C
 17.0 W/m-K
@Temperature 200 °C
 18.0 W/m-K
@Temperature 300 °C
 20.0 W/m-K
@Temperature 400 °C
 21.0 W/m-K
@Temperature 500 °C
 23.0 W/m-K
@Temperature 600 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.030 %
Chromium, Cr 17.5 %
Iron, Fe 64.7 %As Balance
Manganese, Mn 1.7 %
Molybdenum, Mo 2.6 %
Nickel, Ni 13 %
Phosphorus, P <= 0.040 %
Silicon, Si 0.40 %
Sulfur, S <= 0.015 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type 304L Stainless Steel
AISI Type 316L Stainless Steel, annealed strip
AISI Type 316L Stainless Steel, annealed sheet
ATI Allegheny Ludlum Type 316L Stainless Steel, UNS S31603
HP Alloys Nitronic® 50 Austenitic Stainless, Annealed

NSANDV233 / 19127

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.