MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

Proto3000 PC Fused Deposition Modeling Polymer
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: Description: A true industrial thermoplastic, PC (polycarbonate) is widely used in automotive, aerospace, medical and many other applications. PC offers accuracy, durability and stability, creating strong parts that withstand functional testing. A PC part manufactured on a Fortus 3D Production System is 5-60 percent stronger than a part made on previous FDM systems. It also has superior mechanical properties to ABS and a number of other thermoplastics. When combined with a Fortus system, PC gives you Real Parts™ for conceptual modeling, functional prototyping, manufacturing tools, and end-use-parts

Available Colors: White

Information provided by Proto3000 for their protoyping engineering services.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 115115ASTM D785
Tensile Strength at Break 68.0 MPa9860 psiType 1, 2"/min; ASTM D638
Elongation at Break 4.8 %4.8 %ASTM D638
Tensile Modulus 2.28 GPa331 ksiASTM D638
Flexural Strength 104 MPa15100 psiMethod 1, 0.05"/min; ASTM D790
Flexural Modulus 2.234 GPa324.0 ksiASTM D790
Izod Impact, Notched 0.530 J/cm0.993 ft-lb/inMethod A; ASTM D256
Izod Impact, Unnotched 3.20 J/cm5.99 ft-lb/inMethod A; ASTM D256
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant  2.96
@Frequency 1e+6 Hz
2.96
@Frequency 1e+6 Hz
IEC 60250
 3.17
@Frequency 60 Hz
3.17
@Frequency 60 Hz
IEC 60250
Dielectric Strength 15.0 kV/mm381 kV/inIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 38.0 µm/m-°C21.1 µin/in-°FASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 138 °C
@Thickness 0.125 mm
280 °F
@Thickness 0.00492 in
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 127 °C
@Thickness 0.125 mm
261 °F
@Thickness 0.00492 in
ASTM D648
Vicat Softening Point 139 °C282 °FASTM D1525
Glass Transition Temp, Tg 161 °C322 °FDAM (SSYS)
Flammability, UL94 V-2
@Thickness 1.10 mm
V-2
@Thickness 0.0433 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Stratasys® PC Polycarbonate for 3D Printing
Stratasys® ABSi
Stratasys® ABS-M30
Stratasys® ABS-M30i
Stratasys® PC-ABS

PPROTO971 / 133174

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.