MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Ohara S-FPM 4 Optical Glass
Categories: Ceramic; Glass; Optical

Material Notes: S-FPM4 is an optical glass with high partial dispersion ratios ?g, F in the FPM region. The material is very useful for polished lenses that are effective for secondary chromatic aberration correction and these characteristics make it ideal for use in a wide range of applications, such as interchangeable photographic and broadcast lenses as well as automotive lenses. (maximum THK is 35mm)

Information provided by Ohara Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 3.76 g/cc
 
Chemical PropertiesOriginal ValueComments
Acid Class, SR 51.3
 
Mechanical PropertiesOriginal ValueComments
Hardness, Knoop 360
@Load 0.0999 kg
Modulus of Elasticity 74.7 GPa
Modulus of Rigidity 28.9 GPa
Poissons Ratio 0.295
Abrasion 506Aa
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.3 µm/m-°C
@Temperature -30.0 - 70.0 °C
 14.3 µm/m-°C
@Temperature 100 - 300 °C
Thermal Conductivity 0.746 W/m-K
@Temperature 35.0 °C
Transformation Temperature, Tg 488 °Cper thermal expansion curve
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.50911
@Wavelength 2325.42 nm
 1.51254
@Wavelength 1970.09 nm
 1.51625
@Wavelength 1529.58 nm
 1.51955
@Wavelength 1128.64 nm
 1.52065
@Wavelength 1013.98 nm
nt (Hg t line)
 1.52258
@Wavelength 852.11 nm
ns (Cs s line)
 1.5239
@Wavelength 768.19 nm
nA' (K A' line)
 1.5251
@Wavelength 706.52 nm
nr (He r line)
 1.5263
@Wavelength 656.27 nm
nC (H C line)
 1.52664
@Wavelength 643.85 nm
nC' (Cd C' line)
 1.52695
@Wavelength 632.8 nm
nHe-Ne
 1.52835
@Wavelength 589.29 nm
nD
 1.52841
@Wavelength 587.56 nm
nd (He D line)
 1.53006
@Wavelength 546.07 nm
ne (Hg e line)
 1.53321
@Wavelength 486.13 nm
nf (H F line)
 1.53361
@Wavelength 479.99 nm
nF' (Cd F' line)
 1.53645
@Wavelength 441.57 nm
nHe-Cd
 1.53694
@Wavelength 435.835 nm
ng (Hg g line)
 1.54002
@Wavelength 404.656 nm
nh (Hg h line)
 1.54522
@Wavelength 365.015 nm
ni (Hg i line)
Abbe Number 76.07ν e
 76.46ν d
Optical Dispersion 0.002107nd-nC; Partial Dispersion
 0.002406nC-nA'; Partial Dispersion
 0.003076nh-ng; Partial Dispersion
 0.003422ne-nC'; Partial Dispersion
 0.003546nF'-ne; Partial Dispersion
 0.003729ng-nF; Partial Dispersion
 0.003757ne-nC; Partial Dispersion
 0.00565nC-nt; Partial Dispersion
 0.005985nC'-nt; Partial Dispersion
 0.006911nF-nC
 0.006968nF'-nC'
 0.008275ni-ng; Partial Dispersion
 0.008533ng-nd; Partial Dispersion
 0.011612ni-nF'; Partial Dispersion
Transmission, Visible 99.2 %
@Thickness 10.0 mm,
Wavelength 380 nm
Internal Transmission
 99.5 %
@Thickness 10.0 mm,
Wavelength 390 nm
Internal Transmission
 99.5 %
@Thickness 10.0 mm,
Wavelength 420 nm
Internal Transmission
 99.5 %
@Thickness 10.0 mm,
Wavelength 440 nm
Internal Transmission
 99.6 %
@Thickness 10.0 mm,
Wavelength 400 nm
Internal Transmission
 99.6 %
@Thickness 10.0 mm,
Wavelength 460 nm
Internal Transmission
 99.7 %
@Thickness 10.0 mm,
Wavelength 480 nm
Internal Transmission
 99.7 %
@Thickness 10.0 mm,
Wavelength 700 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 500 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 600 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 650 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 550 nm
Internal Transmission
IR Transmittance 99.5 %
@Thickness 10.0 mm,
Wavelength 2400 nm
Internal Transmission
 99.6 %
@Thickness 10.0 mm,
Wavelength 2200 nm
Internal Transmission
 99.7 %
@Thickness 10.0 mm,
Wavelength 800 nm
Internal Transmission
 99.7 %
@Thickness 10.0 mm,
Wavelength 900 nm
Internal Transmission
 99.7 %
@Thickness 10.0 mm,
Wavelength 1000 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 1200 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 1600 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 1800 nm
Internal Transmission
 99.8 %
@Thickness 10.0 mm,
Wavelength 2000 nm
Internal Transmission
 99.9 %
@Thickness 10.0 mm,
Wavelength 1400 nm
Internal Transmission
UV Transmittance 3.0 %
@Thickness 10.0 mm,
Wavelength 280 nm
Internal Transmission
 9.0 %
@Thickness 10.0 mm,
Wavelength 290 nm
Internal Transmission
 20 %
@Thickness 10.0 mm,
Wavelength 300 nm
Internal Transmission
 37 %
@Thickness 10.0 mm,
Wavelength 310 nm
Internal Transmission
 58 %
@Thickness 10.0 mm,
Wavelength 320 nm
Internal Transmission
 75 %
@Thickness 10.0 mm,
Wavelength 330 nm
Internal Transmission
 86 %
@Thickness 10.0 mm,
Wavelength 340 nm
Internal Transmission
 93.4 %
@Thickness 10.0 mm,
Wavelength 350 nm
Internal Transmission
 96.8 %
@Thickness 10.0 mm,
Wavelength 360 nm
Internal Transmission
 98.4 %
@Thickness 10.0 mm,
Wavelength 370 nm
Internal Transmission
 
Descriptive Properties
Acid Resistance, Powder Method, RA(P)3
CCI0.00 B
 0.14 G
 0.14 R
coloring, λ 80340
Coloring, Internal Transmission λ 0.05283
Coloring, Internal Transmission λ 0.80335
Knoop Hardness Class4
Ohara Code d528765
Ohara Code e530760
Phosphate Resistance, PR4.3
Photoelastic Constant (ß)0.72
Water Resistance, RW(P)1
Weathering Resistance (Surface Method) W(S)max1
Yield Point, At (°C)520per thermal expansion curve

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

CZOHARA757 / 281596

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.