MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ THERMOCOMP™ Compound AX06437 Acrylonitrile Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes: LNP THERMOCOMP AX06437 compound is based on Acrylonitrile Butadiene Styrene (ABS) resin containing proprietary fillers. Added features of this grade include: Improved Plating Surface and Mechanical Performance suitable for Laser Direct Structuring (LDS) applications.

Features: Laser Direct Structuring,Circuit Solution

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.17 g/cc1.17 g/cccolor; ASTM D792
Density 1.17 g/cc0.0423 lb/in³ISO 1183
 1.175 g/cc0.04245 lb/in³ASTM D792
Moisture Absorption 0.0500 - 0.100 %0.0500 - 0.100 %Injection Molding
 0.220 %0.220 %23°C/50% RH/24 hrs; ASTM D570
 0.320 %0.320 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0050 cm/cm0.0050 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0060 cm/cm0.0060 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 33.0 MPa4790 psiISO 527
 34.0 MPa4930 psi5 mm/min; ASTM D638
Tensile Strength, Yield 36.0 MPa5220 psiISO 527
 37.0 MPa5370 psi5 mm/min; ASTM D638
Elongation at Break 6.9 %6.9 %5 mm/min; ASTM D638
 7.5 %7.5 %ISO 527
Elongation at Yield 1.8 %1.8 %5 mm/min; ASTM D638
 1.9 %1.9 %ISO 527
Tensile Modulus 3.18 GPa461 ksi5 mm/min; ASTM D638
Flexural Strength 64.0 MPa9280 psiISO 178
 92.0 MPa13300 psibrk, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3.01 GPa437 ksiISO 178
 3.06 GPa444 ksi1.3 mm/min, 50 mm span; ASTM D790
Flexural Strain at Break 64.1 %64.1 %2 mm/min; ISO 178
Izod Impact Notched 26.0 J19.2 ft-lbASTM D256
Izod Impact, Unnotched 2.88 J/cm5.40 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 3.00 kJ/m²1.43 ft-lb/in²80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) 22.0 kJ/m²10.5 ft-lb/in²80*10*3; ISO 180/1U
 22.0 kJ/m²10.5 ft-lb/in²80*10*4; ISO 180/1U
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 2.75
@Frequency 1e+9 Hz
2.75
@Frequency 1e+9 Hz
ASTM D150
Dissipation Factor 0.0024
@Frequency 1e+9 Hz
0.0024
@Frequency 1e+9 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 84.4 µm/m-°C
@Temperature -30.0 - 30.0 °C
46.9 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM E831
CTE, linear, Transverse to Flow 91.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
50.6 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 87.0 °C189 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 86.0 °C
@Thickness 3.20 mm
187 °F
@Thickness 0.126 in
unannealed; ASTM D648
UL RTI, Electrical 60.0 °C140 °FUL 746B
UL RTI, Mechanical with Impact 60.0 °C140 °FUL 746B
UL RTI, Mechanical without Impact 60.0 °C140 °FUL 746B
Flammability, UL94 HB
@Thickness >=1.50 mm
HB
@Thickness >=0.0591 in
UL 94
 
Processing PropertiesMetricEnglishComments
Zone 2 230 - 245 °C446 - 473 °F
Zone 3 265 - 275 °C509 - 527 °F
Melt Temperature 260 °C500 °FInjection Molding
Mold Temperature 70.0 - 80.0 °C158 - 176 °F
Drying Temperature 80.0 °C176 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81474 / 289421

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.