MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

RTP Company RTP 2099 X 145616 PA6/PP; Lubricated - Preliminary Datasheet
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Polypropylene (PP)

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.05 g/cc1.05 g/ccISO 1183
Water Absorption 0.20 %
@Time 86400 sec
0.20 %
@Time 24.0 hour
ASTM D 570
Linear Mold Shrinkage 0.015 - 0.020 cm/cm
@Thickness 4.00 mm
0.015 - 0.020 in/in
@Thickness 0.157 in
ISO 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 60.0 MPa8700 psiISO 527
Elongation at Break >= 10 %>= 10 %ISO 527
Tensile Modulus 2.60 GPa377 ksiISO 527
Flexural Strength 80.0 MPa11600 psiISO 178
Flexural Modulus 2.30 GPa334 ksiISO 178
Izod Impact, Notched (ISO) 7.00 kJ/m²
@Thickness 4.00 mm
3.33 ft-lb/in²
@Thickness 0.157 in
ISO 180/1A
Izod Impact, Unnotched (ISO) 100 kJ/m²
@Thickness 4.00 mm
47.6 ft-lb/in²
@Thickness 0.157 in
ISO 180/1U
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FISO 75
Vicat Softening Point 147 °C297 °F120°C/hr; 50N; ISO 306
 
Processing PropertiesMetricEnglishComments
Melt Temperature 232 - 260 °C450 - 500 °F
Mold Temperature 54.0 - 82.0 °C129 - 180 °F
Drying Temperature 80.0 °C
@Time 7200 sec
176 °F
@Time 2.00 hour
Moisture Content 0.20 %0.20 %
Injection Pressure 69.0 - 103 MPa10000 - 14900 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene, Molded
Avient Maxxam™ NT-818.B001-8000 Polypropylene
Avient Maxxam™ NT-818.B001-7001 Polypropylene
Avient Edgetek® 5209 Black 30 A 1 Acetal (POM) Copolymer

PQZRA39537 / 205945

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.