MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
446 Stainless Steel, Soft Tempered Wire
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Properties below for 6.4 mm (1/4 in.) diameter wire. The excellent corrosion resistance of this non-hardenable, ferritic stainless is due to the high chromium content. This allows use in applications such as heaters, burners, nozzles, electrodes, and metal-ceramic seals. Typical annealing temperatures are 730-815°C; followed by air or water quench.

Key Words: ASME SA268; ASTM A176; ASTM A276; ASTM A314; ASTM A473; ASTM A511; ASTM A580, UNS S44600; FED QQ-S-763; FED QQ-S-766; Mil Spec MIL-S-862; SAE J405 (51466)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 195Estimated from Rockwell B
Hardness, Knoop 211Estimated from Rockwell B
Hardness, Rockwell A 56.4Estimated from Rockwell B
Hardness, Rockwell B 92
Hardness, Vickers 195Estimated from Rockwell B
Tensile Strength, Ultimate 655 MPa
Tensile Strength, Yield 550 MPa
@Strain 0.2 %
Elongation at Break 15 %in 25 mm
Reduction of Area 50 %
Modulus of Elasticity 200 GPaAnnealed
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000640 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.4 µm/m-°C
@Temperature 0.000 - 100 °C
 10.8 µm/m-°C
@Temperature 0.000 - 315 °C
 11.2 µm/m-°C
@Temperature 0.000 - 540 °C
 11.5 µm/m-°C
@Temperature 0.000 - 650 °C
 12.1 µm/m-°C
@Temperature 0.000 - 980 °C
Specific Heat Capacity 0.460 J/g-°C
Thermal Conductivity 21.6 W/m-K
 24.6 W/m-K
@Temperature 500 °C
Melting Point 1425 - 1510 °C
Solidus 1425 °C
Liquidus 1510 °C
Maximum Service Temperature, Air 1095 °COxidation resistant for service up to 1095°C. Mechanical properties suffer below this point.
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.20 %
Chromium, Cr 23 - 27 %
Iron, Fe 75 %As remainder
Manganese, Mn <= 1.5 %
Nickel, Ni <= 0.25 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
446 Stainless Steel, Annealed Bar
446 Stainless Steel, Annealed Sheet
446 Stainless Steel, Annealed and Cold Drawn Bar
446 Stainless Steel, Annealed Plate
446 Stainless Steel, Annealed Strip

MQ446A2 / 13217

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.