MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Polykemi AB POLYelast TPE Z800 Thermoplastic Elastomer, SEBS-based
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes:

Information provided by Polykemi AB

Key Words: Thermoplastic Elastomer, SEBS
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.900 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.017 - 0.024 cm/cmISO 2577
Linear Mold Shrinkage, Transverse 0.017 - 0.024 cm/cmISO 2577
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 80
@Time 15.0 sec
Polykemi
Tensile Strength at Break <= 12.0 MPaISO/R527
Elongation at Break 500 %ISO/R527
100% Modulus 0.00380 GPa
@Strain 100 %
ISO/R527
300% Modulus 0.00530 GPa
@Strain 300 %
ISO/R527
Tear Strength 26.0 kN/mD624
 
Processing PropertiesOriginal ValueComments
Melt Temperature 180 - 220 °C
Mold Temperature 20.0 - 40.0 °C
Back Pressure 0.500 - 1.50 MPa
 
Descriptive Properties
Holding PressureLow
Injection PressureLow
Injection SpeedHigh

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPOLYK489 / 123214

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.