MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Syensqo (Solvay Specialty Polymers) Amodel® AT-6130 HS PPA, 30% glass fiber
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 30% Glass Fiber Reinforced

Material Notes: 30% glass fiber, impact modified, high flow, hot-water molds, heat stabilized

Amodel® AT-6130 HS is a 30% glass-reinforced, toughened polyphthalamide (PPA) resin that has more elongation than other 30% glass-reinforced grades of Amodel® resin. This grade was developed for automotive snap-fit electronic connectors. It offers high flow and short molding cycles. The processing window is relatively broad and mold temperatures as low as 150°F (65°C) can be used.

- Black: AT-6130 HS BK 324
- Natural: AT-6130 HS NT

Applications: Automotive Applications; Automotive Electronics; Automotive Under the Hood; Bearings; Connectors; Fuel Lines; General Purpose; Housings; Industrial Applications; Industrial Parts; Lawn and Garden Equipment; Machine/Mechanical Parts; Metal Replacement; Valves/Valve Parts

Features: Chemical Resistant; Good Flow; Heat Stabilized; High Heat Resistance; High Strength; Hot Water Moldability; Impact Modified; Low Friction; Lubricated; Wear Resistant

Injection notes: Injection pressure between 2-4 in/sec (5-10 cm/sec). Adjust the holding pressure to one-half the injection pressure.
Storage:
- Amodel® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Amodel® resins be dried prior to molding following the recommendations found in this datasheet and/or in the Amodel® processing guide.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.34 g/cc0.0484 lb/in³Method A; ISO 1183
Water Absorption 0.15 %
@Time 86400 sec
0.15 %
@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0050 cm/cm0.0050 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 167 MPa24200 psiASTM D638
 170 MPa24700 psiISO 527-2
Elongation at Break 3.2 %3.2 %ASTM D638
 3.3 %3.3 %ISO 527-2
Tensile Modulus 9.31 GPa1350 ksiISO 527-2
Flexural Strength 225 MPa32600 psiISO 178
Flexural Yield Strength 236 MPa34200 psiASTM D790
Flexural Modulus 7.58 GPa1100 ksiISO 178
 7.86 GPa1140 ksiASTM D790
Izod Impact, Notched 1.30 J/cm2.44 ft-lb/inASTM D256
Izod Impact, Unnotched 14.0 J/cm26.2 ft-lb/inASTM D256
Charpy Impact, Notched 1.30 J/cm²6.19 ft-lb/in²Type 1, Edgewise, Notch A; ISO 179
 
Thermal PropertiesMetricEnglishComments
Melting Point 306 °C583 °FPeak; ASTM D3418
 310 °C590 °FISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 298 °C568 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 276 °C529 °FUnannealed; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 316 - 324 °C601 - 615 °F
Front Barrel Temperature 327 - 332 °C621 - 630 °F
Melt Temperature 321 - 335 °C610 - 635 °FInjection
Mold Temperature 66.0 - 93.0 °C151 - 199 °F
Drying Temperature 121 °C
@Time 14400 sec
250 °F
@Time 4.00 hour
Moisture Content 0.030 - 0.060 %0.030 - 0.060 %Injection
 
Descriptive Properties
AdditiveHeat Stabilizer; Impact Modifier; Lubricant; Mold Release
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorBlack; Natural Color
FormsPellets
Injection RateFast
ProcessingWater-Heated Mold Injection Molding
RoHS ComplianceYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4107 / 279907

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.