MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Celanex® 3300-2FC PBT, 30% Glass Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled

Material Notes: Celanex 3300-2FC is a general purpose, 30% glass reinforced, polybutylene terephthalate that offers a superior combination of mechanical, electrical, and thermal properties. This grade provides outstanding processability and good chemical resistance. Celanex 3300-2FC is a high flow material that contains an internal lubricant.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.53 g/ccASTM D792
Density 1.53 g/ccISO 1183
Water Absorption 0.070 %
@Temperature 22.8 °C
24hr immersion; ASTM D570
Moisture Absorption 0.200 %23°C/50%RH; ISO 62
Viscosity Test 74 cm³/gISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cmASTM D955
 0.0030 - 0.0070 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0070 - 0.011 cm/cmISO 294-4
Melt Flow 16 g/10 minASTM D1238
 17 g/10 min
@Load 2.16 kg,
Temperature 250 °C
[cm3/10min]; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 90ISO 2039-2
Tensile Strength at Break 130 MPa5mm/min; ISO 527-2/1A
 19500 psiASTM D638
 8900 psi
@Temperature 121 °C
ASTM D638
 11250 psi
@Temperature 80.0 °C
ASTM D638
 23000 psi
@Temperature 0.000 °C
ASTM D638
 27500 psi
@Temperature -40.0 °C
ASTM D638
Elongation at Break 2.0 %ASTM D638
 2.5 %5mm/min; ISO 527-2/1A
 1.9 %
@Temperature 0.000 °C
ASTM D638
 1.9 %
@Temperature 4.44 °C
ASTM D638
 3.9 %
@Temperature 80.0 °C
ASTM D638
 4.3 %
@Temperature 121 °C
ASTM D638
Tensile Modulus 9200 MPa50mm/min; ISO 527-2/1A
 1.40e+6 psiASTM D638
 545000 psi
@Temperature 121 °C
ASTM D638
 700000 psi
@Temperature 80.0 °C
ASTM D638
 1.52e+6 psi
@Temperature 0.000 °C
ASTM D638
 1.60e+6 psi
@Temperature -40.0 °C
ASTM D638
Flexural Strength 210 MPaISO 178
 28000 psiASTM D790
Flexural Modulus 9700 MPaISO 178
 1.20e+6 psiASTM D790
Izod Impact, Notched 1.70 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 7.50 kJ/m²ISO 180/1A
Charpy Impact Unnotched 46.0 kJ/m²ISO 179/1eU
 45.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 8.50 kJ/m²ISO 179/1eA
 8.50 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
 1.00e+15 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.7
@Frequency 1e+6 Hz
ASTM D150
 4.1
@Frequency 1e+6 Hz
IEC 60250
 4.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 31.0 kV/mmIEC 60243-1
 560 V/milshort term; ASTM D149
Dissipation Factor 0.0020
@Frequency 1e+6 Hz
ASTM D150
 0.0022
@Frequency 100 Hz
IEC 60250
 0.016
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 425 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 25.0 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 100 µm/m-°CISO 11359-2
Melting Point 225 °C10°C/min; ISO 11357-1,-2,-3
 437 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 225 °CISO 75-1, -2
 442 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 205 °CISO 75-1, -2
 403 °FASTM D648
Deflection Temperature at 8.0 MPa 150 °CISO 75-1, -2
Vicat Softening Point 220 °CISO 306
Glass Transition Temp, Tg 60.0 °CISO 11357-1,-2,-3
Flammability, UL94 HB
@Thickness 0.710 mm
Oxygen Index 20 %ISO 4589
 
Processing PropertiesOriginal ValueComments
Processing Temperature 65.0 - 93.0 °Ccavity
 250 - 260 °Chot runner
Feed Temperature 230 - 240 °C
Zone 1 230 - 240 °C
Zone 2 235 - 250 °C
Zone 3 235 - 250 °C
Zone 4 240 - 260 °C
Die Temperature 250 - 260 °C
Melt Temperature 235 - 260 °C
 260 °CISO 294
Mold Temperature 82.0 °CISO 294
Injection Velocity 300 mm/secISO 294
Drying Temperature 120 - 130 °C
Dry Time 4.00 hour
Moisture Content <= 0.020 %
Hold Pressure 48.0 MPaISO 294
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Processing conditions acc. ISO7792-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mitsubishi Novaduran® 5010GN6-30M8X Polybutylene Terephthalate
Mitsubishi Novaduran® 5010GN6-30T Polybutylene Terephthalate
Celanese Celanex® 3300 PBT, 30% Glass Reinforced
Celanese Celanex® 3300-2 PBT, 30% Glass Reinforced
Celanese Celanex® 3300-2LM PBT, Glass Reinforced

PHCQ048 / 178503

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.