MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Texin® RxT85A Thermoplastic Polyurethanes (TPU)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Characterization: Texin RxT85A resin is an aromatic polyether-based thermoplastic polyurethane. It can be processed by injection molding, extrusion or blow molding.

Properties / Applications: Texin RxT85A offers outstanding abrasion resistance, impact strength, toughness and flexibility. It also exhibits excellent hydrolytic stability. Typical medical applications include anesthetic connectors, catheters, flexible tubing, film, seals and gaskets and extruded profiles. As with any product, the use of Texin RxT85A resin in a given application must be tested (including but not limited to field testing) in advance by the user to determine suitability.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.12 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
Melt Flow 4.0 g/10 min
@Load 8.70 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 85ASTM D2240
Tensile Strength at Break 36.6 MPaASTM D412
Tensile Stress at Strain 5.50 MPa
@Strain 100 %
ASTM D412
 9.70 MPa
@Strain 300 %
ASTM D412
Elongation at Break 610 %ASTM D412
Flexural Modulus 26.9 MPaASTM D790
Tear Strength 87.6 kN/mDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 30
@Load 1.00 kg
[mg] Loss, H-18; ASTM D3489
Compression Set 16 %
@Temperature 23.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 40 %
@Temperature 70.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 80.0 °CRate A; ASTM D1525
 
Optical PropertiesOriginal ValueComments
Yellow Index <= 10 %ASTM E313
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 182 - 193 °CExtrusion
 193 - 204 °CInjection
Middle Barrel Temperature 193 - 204 °CExtrusion
 196 - 207 °CInjection
Front Barrel Temperature 193 - 204 °CExtrusion
 196 - 207 °CInjection
Nozzle Temperature 199 - 210 °CInjection
Die Temperature 193 - 210 °CExtrusion
Melt Temperature 199 - 210 °CInjection
 199 - 210 °CExtrusion
Mold Temperature 16.0 - 38.0 °CInjection
Injection Pressure 6000 - 15000 psiInjection
Back Pressure <= 800 psiInjection
Cushion <= 0.125 inInjection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Elastollan® C-85A Polyester Type Polyurethane Elastomer
Lubrizol Pellethane® 2363-90AE Thermoplastic Polyurethane Elastomer
Arkema Pebax® 3533 SA 01 MED Polyether Block Amide (PEBA)
Lubrizol LifeSciences Tecoflex® EG-93A-B40 TPU – 40% Barium Sulfate
AorTech Biomaterials ECSil™ 90A Biomedical Carbonate Silicone Pellets

PCOVEST0998 / 202781

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.