MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Ascend Performance Materials Vydyne® 41 NT Impact Modified Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Impact Grade

Material Notes: Vydyne 41 NT is a general-purpose, high impact-modified PA66 resin. The product is recognized for all the processing and property advantages inherent to PA66 with the addition of improved impact strength. This resin offers a well balanced combination of engineering properties characterized by high melt point, good surface lubricity, abrasion resistance and resistance to many chemicals, machine and motor oils, solvents and gasoline. 41 NT is designed to meet the critical low-temperature impact requirements called out in many automotive specifications.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.08 g/ccDAM; ISO 1183
Water Absorption 1.0 %
@Time 86400 sec
DAM; ISO 62
Moisture Absorption at Equilibrium 2.1 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.018 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.016 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 39.0 MPa50% RH; ISO 527-2
 43.0 MPaDAM; ISO 527-2
Tensile Strength, Yield 35.0 MPa50% RH; ISO 527-2
 50.0 MPaDAM; ISO 527-2
Elongation at Break 50 %DAM; ISO 527-2
 175 %50% RH; ISO 527-2
Tensile Modulus 1400 MPa50% RH; ISO 527-2
 2200 MPaDAM; ISO 527-2
Flexural Strength 17.0 MPa50% RH; ISO 178
 53.0 MPaDAM; ISO 178
Flexural Modulus 500 MPa50% RH; ISO 178
 1800 MPaDAM; ISO 178
Izod Impact, Notched (ISO) 29.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 40.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 78.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 88.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched NB
@Temperature -30.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature -30.0 °C
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 25.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 35.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 76.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 110 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+11 ohm-cm
@Thickness 1.00 mm
DAM; IEC 60093
Dielectric Strength 26.0 kV/mm
@Thickness 1.00 mm
DAM; IEC 60243
Arc Resistance 120 - 180 sec
@Thickness 3.00 mm
PLC 5; ASTM D 495
Comparative Tracking Index 600 V
@Thickness 3.00 mm
IEC 60112
Hot Wire Ignition, HWI 7.0 - 15 secPLC 4; UL 746
 15 - 30 secPLC 3; UL 746
 15 - 30 secPLC 3; UL 746
High Amp Arc Ignition, HAI >= 120 arcsPLC 0; UL 746
 >= 120 arcsPLC 0; UL 746
 >= 120 arcsPLC 0; UL 746
High Voltage Arc-Tracking Rate, HVTR 0.000 - 10.0 mm/minUL 746
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 168 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 149 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
DAM; ISO 11359-2
Melting Point 260 °CDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 145 °CUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 58.0 °CUnannealed; DAM; ISO 75-2/A
UL RTI, Electrical 125 °C
@Thickness 0.750 mm
UL 746
 125 °C
@Thickness 1.50 mm
UL 746
 125 °C
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical with Impact 75.0 °C
@Thickness 0.750 mm
UL 746
 75.0 °C
@Thickness 1.50 mm
UL 746
 75.0 °C
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical without Impact 85.0 °C
@Thickness 0.750 mm
UL 746
 85.0 °C
@Thickness 1.50 mm
UL 746
 85.0 °C
@Thickness 3.00 mm
UL 746
Flammability, UL94 HB
@Thickness 0.750 mm
 HB
@Thickness 1.50 mm
 HB
@Thickness 3.00 mm
Glow Wire Ignition Temperature 725 °C
@Thickness 0.750 mm
IEC 60695-2-13
 725 °C
@Thickness 1.50 mm
IEC 60695-2-13
 775 °C
@Thickness 0.400 mm
IEC 60695-2-13
Glow Wire Flammability Index 700 °C
@Thickness 0.750 mm
IEC 60695-2-12
 700 °C
@Thickness 1.50 mm
IEC 60695-2-12
 750 °C
@Thickness 0.400 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 280 - 310 °CInjection
Middle Barrel Temperature 280 - 310 °CInjection
Front Barrel Temperature 280 - 310 °CInjection
Nozzle Temperature 280 - 310 °CInjection
Melt Temperature 285 - 305 °CInjection
Mold Temperature 65.0 - 95.0 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 4.00 hourInjection
 
Descriptive Properties
Agency RatingsASTM, D4066 PA0171
 ASTM, D6779 PA0171
AppearanceNatural Color
FeaturesAbrasion Resistance
 Chemical Resistant
 Gasoline Resistant
 Good Processability
 High Impact Resistance
 Impact Modified
 Low Temperature Impact Resistance
 Oil Resistant
 Solvent Resistant
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Nylene® Nylene 4114 Nylon 66, Impact Grade
Wellman Wellamid® XT1573-N Impact Modified Nylon 66
Ascend Performance Materials Vydyne® 47 NT Impact Modified Nylon 66
Envalior Akulon® K224-PG6 PA6-I-GF30, Dry, 30% Glass Reinforced, Impact Modified
Celanese Zytel® ST801A NC010A PA66-HI

PASCE9701 / 220804

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.