MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
MAR-M302 Cast Cobalt Alloy
Categories: Metal; Superalloy; Cobalt Base

Material Notes: Typical applications: jet engine blades, vanes

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 9.21 g/cc
 
Mechanical PropertiesOriginal ValueComments
Rupture Strength 4000 psi
@Temperature 1090 °C,
Time 3.60e+6 sec
 6000 psi
@Temperature 1090 °C,
Time 360000 sec
 11000 psi
@Temperature 982 °C,
Time 3.60e+6 sec
 16000 psi
@Temperature 982 °C,
Time 360000 sec
 30000 psi
@Temperature 816 °C,
Time 3.60e+6 sec
 40000 psi
@Temperature 816 °C,
Time 360000 sec
 
Component Elements PropertiesOriginal ValueComments
Boron, B 0.0050 %
Carbon, C 0.85 %
Chromium, Cr 21.5 %
Cobalt, Co 58.195 %Balance
Manganese, Mn 0.10 %
Silicon, Si 0.20 %
Tantalum, Ta 9.0 %
Tungsten, W 10 %
Zirconium, Zr 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
MAR-M509 Cast Cobalt Alloy
WI-52 Cast Cobalt Alloy
S-816 Cobalt Alloy, UNS R30816
MAR-M918 Cobalt Alloy
MAR-M432 Cast Nickel Superalloy

NZ97078 / 191471

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.