MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Polycarbonate/ABS Alloy, Unreinforced
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polycarbonate/ABS Alloy, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.960 - 1.50 g/ccAverage value: 1.16 g/cc Grade Count:1105
 0.935 - 1.01 g/cc
@Temperature 240 - 260 °C
Average value: 0.981 g/cc Grade Count:10
Filler Content 10.0 %Average value: 10.0 % Grade Count:3
Volatile Organic Compounds (VOC) Content 9.00 - 15.0 g/lAverage value: 11.1 g/l Grade Count:10
Water Absorption 0.0100 - 0.700 %Average value: 0.295 % Grade Count:305
Moisture Absorption at Equilibrium 0.0100 - 0.900 %Average value: 0.162 % Grade Count:244
Water Absorption at Saturation 0.110 - 1.00 %Average value: 0.555 % Grade Count:118
Viscosity 105000 - 211000 cP
@Temperature 260 - 260 °C
Average value: 141000 cP Grade Count:4
 8.00 - 41.0 cP
@Temperature 260 - 265 °C
Average value: 141000 cP Grade Count:33
 8.00 - 41.0 cP
@Load 2.16 - 10.0 kg
Average value: 141000 cP Grade Count:33
 150000 - 520000 cP
@Temperature 260 - 260 °C
Average value: 141000 cP Grade Count:12
 150000 - 520000 cP
@Frequency 1000 - 1000 Hz
Average value: 141000 cP Grade Count:12
 170 - 2.00e+6 cP
@Temperature 260 - 260 °C
Average value: 141000 cP Grade Count:38
 170 - 2.00e+6 cP
@Shear Rate 1000 - 1500 1/s
Average value: 141000 cP Grade Count:38
Maximum Moisture Content 0.0100 - 0.0500Average value: 0.0218 Grade Count:74
Linear Mold Shrinkage 0.000600 - 0.0800 cm/cmAverage value: 0.00565 cm/cm Grade Count:833
 0.00700 - 0.00700 cm/cm
@Temperature 80.0 - 80.0 °C
Average value: 0.00700 cm/cm Grade Count:3
Linear Mold Shrinkage, Transverse 0.000600 - 0.0100 cm/cmAverage value: 0.00564 cm/cm Grade Count:223
 0.00700 - 0.00700 cm/cm
@Temperature 80.0 - 80.0 °C
Average value: 0.00700 cm/cm Grade Count:3
Melt Flow 0.400 - 95.0 g/10 minAverage value: 18.5 g/10 min Grade Count:945
Spiral Flow 25.0 - 76.0 cmAverage value: 52.6 cm Grade Count:17
 47.0 - 58.0 cm
@Temperature 260 - 260 °C
Average value: 47.2 cm Grade Count:4
 24.7 - 63.0 cm
@Temperature 260 - 260 °C
Average value: 47.2 cm Grade Count:5
 24.7 - 63.0 cm
@Thickness 2.00 - 2.00 mm
Average value: 47.2 cm Grade Count:5
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 72.0 - 97.0Average value: 90.4 Grade Count:8
Hardness, Rockwell R 98.0 - 123Average value: 115 Grade Count:297
Hardness, Shore A 45.0 - 85.0Average value: 63.2 Grade Count:11
Hardness, Shore D 62.0 - 85.0Average value: 70.7 Grade Count:6
Hardness, Shore M 30.0 - 95.0Average value: 55.0 Grade Count:3
Ball Indentation Hardness 12.0 - 126 MPaAverage value: 98.2 MPa Grade Count:25
Tensile Strength, Ultimate 2.80 - 586 MPaAverage value: 53.3 MPa Grade Count:568
 20.0 - 45.0 MPa
@Temperature 60.0 - 90.0 °C
Average value: 32.5 MPa Grade Count:1
Tensile Strength, Yield 5.00 - 119 MPaAverage value: 56.3 MPa Grade Count:826
Elongation at Break 0.800 - 1230 %Average value: 68.9 % Grade Count:813
 45.0 - 55.0 %
@Temperature 60.0 - 90.0 °C
Average value: 50.0 % Grade Count:1
Elongation at Yield 1.90 - 80.0 %Average value: 5.48 % Grade Count:363
 4.00 - 6.00 %
@Temperature 60.0 - 90.0 °C
Average value: 5.00 % Grade Count:1
Modulus of Elasticity 1.67 - 11.1 GPaAverage value: 2.60 GPa Grade Count:510
 1.90 - 2.20 GPa
@Temperature 60.0 - 90.0 °C
Average value: 2.05 GPa Grade Count:1
Flexural Yield Strength 8.20 - 900 MPaAverage value: 88.1 MPa Grade Count:798
Flexural Modulus 0.290 - 23.1 GPaAverage value: 2.57 GPa Grade Count:899
Flexural Strain at Break 1.30 - 6.10 %Average value: 4.15 % Grade Count:4
Compressive Yield Strength 53.0 - 170 MPaAverage value: 84.5 MPa Grade Count:6
Bearing Yield Strength 25.2 - 293 MPaAverage value: 134 MPa Grade Count:5
Poissons Ratio 0.340 - 0.380Average value: 0.353 Grade Count:9
Shear Strength 40.3 - 61.9 MPaAverage value: 54.3 MPa Grade Count:5
Izod Impact 37.0 - 824 JAverage value: 511 J Grade Count:50
 37.0 - 480 J
@Temperature -30.0 - -30.0 °C
Average value: 172 J Grade Count:31
Izod Impact, Notched 0.196 - 56.0 J/cmAverage value: 5.31 J/cm Grade Count:625
 0.600 - 6.40 J/cm
@Temperature -50.0 - 0.000 °C
Average value: 3.48 J/cm Grade Count:115
 1.01441 - 5.34 J/cm
@Temperature -40.0 - 0.000 °C
Average value: 3.48 J/cm Grade Count:49
 1.01441 - 5.34 J/cm
@Thickness 3.17 - 6.35 mm
Average value: 3.48 J/cm Grade Count:49
Izod Impact, Unnotched 0.530 J/cm - NBAverage value: 7.05 J/cm Grade Count:84
 2.00 J/cm - NB
@Temperature -30.0 - 0.000 °C
Average value: 4.66 J/cm Grade Count:16
Izod Impact, Notched (ISO) 1.80 - 80.0 kJ/m²Average value: 38.7 kJ/m² Grade Count:272
 4.00 - 61.0 kJ/m²
@Temperature -40.0 - 0.000 °C
Average value: 22.3 kJ/m² Grade Count:159
 15.0 - 35.7 kJ/m²
@Temperature -30.0 - -30.0 °C
Average value: 22.3 kJ/m² Grade Count:2
 15.0 - 35.7 kJ/m²
@Thickness 3.17 - 3.20 mm
Average value: 22.3 kJ/m² Grade Count:2
Izod Impact, Unnotched (ISO) 3.00 kJ/m² - NBAverage value: 52.1 kJ/m² Grade Count:86
 21.0 kJ/m² - NB
@Temperature -30.0 - -30.0 °C
Average value: 109 kJ/m² Grade Count:38
Charpy Impact Unnotched 0.290 J/cm² - NBAverage value: 9.66 J/cm² Grade Count:180
 3.50 J/cm² - NB
@Temperature -40.0 - -20.0 °C
Average value: 16.8 J/cm² Grade Count:54
Charpy Impact, Notched 0.0900 - 11.0 J/cm²Average value: 3.98 J/cm² Grade Count:330
 0.500 - 6.00 J/cm²
@Temperature -40.0 - 0.000 °C
Average value: 2.23 J/cm² Grade Count:175
 3.57 - 3.57 J/cm²
@Temperature -30.0 - -30.0 °C
Average value: 2.23 J/cm² Grade Count:1
 3.57 - 3.57 J/cm²
@Thickness 3.20 - 3.20 mm
Average value: 2.23 J/cm² Grade Count:1
Gardner Impact 4.52 - 71.4 JAverage value: 38.3 J Grade Count:37
 59.0 - 59.0 J
@Temperature -29.0 - -29.0 °C
Average value: 65.7 J Grade Count:2
Dart Drop, Total Energy 11.0 - 90.0 JAverage value: 54.2 J Grade Count:100
 8.00 - 90.0 J
@Temperature -30.0 - -28.9 °C
Average value: 53.3 J Grade Count:33
 56.5 - 59.9 J
@Temperature -29.0 - -29.0 °C
Average value: 53.3 J Grade Count:2
 56.5 - 59.9 J
@Thickness 3.20 - 3.20 mm
Average value: 53.3 J Grade Count:2
Falling Dart Impact 6.78 - 60.0 JAverage value: 41.3 J Grade Count:8
 50.1653 - 50.1653 J
@Temperature -28.9 - -28.9 °C
Average value: 50.2 J Grade Count:1
Instrumented Impact Total Energy 4.00 - 62.2 JAverage value: 49.3 J Grade Count:16
Puncture Energy 44.0 - 51.0 JAverage value: 46.3 J Grade Count:6
 20.0 - 57.0 J
@Temperature -30.0 - -30.0 °C
Average value: 47.0 J Grade Count:6
Coefficient of Friction 0.160 - 0.370Average value: 0.246 Grade Count:7
Coefficient of Friction, Static 0.0500 - 0.180Average value: 0.142 Grade Count:5
Tensile Creep Modulus, 1 hour 1800 - 2500 MPaAverage value: 2140 MPa Grade Count:5
Tensile Creep Modulus, 1000 hours 1500 - 1900 MPaAverage value: 1720 MPa Grade Count:5
K (wear) Factor 14.1 - 2520 x 10-8 mm³/N-MAverage value: 754 x 10-8 mm³/N-M Grade Count:4
Taber Abrasion, mg/1000 Cycles 54.0 - 82.0Average value: 64.4 Grade Count:7
Compression Set 21.0 - 45.0 %Average value: 32.3 % Grade Count:11
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 100 - 1.00e+18 ohm-cmAverage value: 4.91e+16 ohm-cm Grade Count:297
Surface Resistance 10.0 - 5.00e+17 ohmAverage value: 1.08e+16 ohm Grade Count:278
Static Decay 0.0100 - 0.250 secAverage value: 0.0580 sec Grade Count:5
Shielding Effectiveness 47.0 - 70.0 dBAverage value: 54.9 dB Grade Count:3
Dielectric Constant 2.00 - 3.40Average value: 2.93 Grade Count:166
Dielectric Strength 2.76 - 70.0 kV/mmAverage value: 28.1 kV/mm Grade Count:222
Dissipation Factor 0.00100 - 0.0150Average value: 0.00588 Grade Count:150
Arc Resistance 60.0 - 180 secAverage value: 112 sec Grade Count:51
Comparative Tracking Index 175 - 650 VAverage value: 331 V Grade Count:183
Hot Wire Ignition, HWI 7.00 - 120 secAverage value: 42.5 sec Grade Count:60
High Amp Arc Ignition, HAI 30.0 - 120 arcsAverage value: 108 arcs Grade Count:52
High Voltage Arc-Tracking Rate, HVTR 25.4 - 150 mm/minAverage value: 115 mm/min Grade Count:20
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.00 - 110 µm/m-°CAverage value: 71.0 µm/m-°C Grade Count:353
 -60.0 - 74.0 µm/m-°C
@Temperature 29.0 - 100 °C
Average value: 17.1 µm/m-°C Grade Count:5
CTE, linear, Transverse to Flow 8.00 - 105 µm/m-°CAverage value: 74.6 µm/m-°C Grade Count:197
 8.30 - 80.0 µm/m-°C
@Temperature 40.0 - 100 °C
Average value: 32.2 µm/m-°C Grade Count:3
Specific Heat Capacity 1.23 - 2.54 J/g-°CAverage value: 1.78 J/g-°C Grade Count:16
Thermal Conductivity 0.142 - 1.70 W/m-KAverage value: 0.222 W/m-K Grade Count:68
 0.240 - 0.260 W/m-K
@Temperature 30.0 - 280 °C
Average value: 0.250 W/m-K Grade Count:2
Melting Point 130 - 270 °CAverage value: 219 °C Grade Count:6
Maximum Service Temperature, Air 60.0 - 132 °CAverage value: 103 °C Grade Count:45
Hot Ball Pressure Test 75.0 - 125 °CAverage value: 94.3 °C Grade Count:84
Deflection Temperature at 0.46 MPa (66 psi) 53.9 - 250 °CAverage value: 112 °C Grade Count:504
Deflection Temperature at 1.8 MPa (264 psi) 52.0 - 160 °CAverage value: 101 °C Grade Count:929
Vicat Softening Point 38.1 - 230 °CAverage value: 117 °C Grade Count:628
 97.0 - 136 °C
@Temperature 50.0 - 50.0 °C
Average value: 119 °C Grade Count:8
 97.0 - 136 °C
@Load 5.10 - 5.10 kg
Average value: 119 °C Grade Count:8
Minimum Service Temperature, Air -50.0 - -40.0 °CAverage value: -41.3 °C Grade Count:15
Glass Transition Temp, Tg 94.0 - 161 °CAverage value: 123 °C Grade Count:12
UL RTI, Electrical 60.0 - 105 °CAverage value: 74.5 °C Grade Count:135
UL RTI, Mechanical with Impact 60.0 - 100 °CAverage value: 71.7 °C Grade Count:136
UL RTI, Mechanical without Impact 60.0 - 105 °CAverage value: 74.1 °C Grade Count:136
Flammability, UL94 HB - 5VAGrade Count:785
Flame Spread 5.00 - 50.0 mm/minAverage value: 25.2 mm/min Grade Count:5
Smoke Density 40.0 - 225Average value: 138 Grade Count:3
Oxygen Index 20.0 - 35.0 %Average value: 27.2 % Grade Count:92
Glow Wire Test 550 - 960 °CAverage value: 833 °C Grade Count:132
 
Optical PropertiesOriginal ValueComments
Gloss 2.50 - 105 %Average value: 55.3 % Grade Count:11
Transmission, Visible 0.100 - 93.0 %Average value: 23.4 % Grade Count:3
 
Processing PropertiesOriginal ValueComments
Processing Temperature 60.0 - 302 °CAverage value: 205 °C Grade Count:131
Nozzle Temperature 220 - 330 °CAverage value: 261 °C Grade Count:280
Adapter Temperature 210 - 270 °CAverage value: 235 °C Grade Count:4
Die Temperature 210 - 265 °CAverage value: 241 °C Grade Count:6
Melt Temperature 180 - 330 °CAverage value: 255 °C Grade Count:588
Mold Temperature 26.7 - 150 °CAverage value: 72.9 °C Grade Count:619
Injection Velocity 40.0 - 240 mm/secAverage value: 237 mm/sec Grade Count:67
Roll Temperature 65.0 - 100 °CAverage value: 81.7 °C Grade Count:3
Drying Temperature 21.1 - 140 °CAverage value: 92.6 °C Grade Count:565
Moisture Content 0.0100 - 0.300 %Average value: 0.0331 % Grade Count:200
Dew Point -40.0 - -17.8 °CAverage value: -28.9 °C Grade Count:14
Drying Air Flow Rate 22.7 - 28.3 l/minAverage value: 25.5 l/min Grade Count:3
Injection Pressure 4.96 - 150 MPaAverage value: 94.1 MPa Grade Count:69
Vent Depth 0.00300 - 0.00762 cmAverage value: 0.00536 cm Grade Count:84
Cushion 0.330 - 0.635 cmAverage value: 0.483 cm Grade Count:3
Precipitation Temperature 60.0 - 80.0 °CAverage value: 70.0 °C Grade Count:22

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Overview of materials for Polycarbonate/ABS Alloy, Glass Fiber Filled
Overview of materials for Polycarbonate, Molded
Overview of materials for Polycarbonate/ABS Alloy, Carbon Fiber Filled
Overview of materials for PC/ABS + Stainless Steel

O1170a / 89060

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.