MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Sarlink® TPV 2774N XRD1 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 2774N XRD1 is a high performance thermoplastic vulcanizate used in automotive applications. Sarlink TPV 2774N XRD1 is a medium hardness, low density, lubricated grade exhibiting sunlight resistance and UV absorbing characteristics. This grade can be processed by injection molding and extrusion.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Filled; Light Stabilized; Low Density; Medium Hardness; Low Specific Gravity; Low Flow; Lubricated; Slip; Sunlight Resistant; UV Absorbing

Uses: Automotive Exterior Trim; Automotive Interior Parts; Automotive Interior Trim

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion; Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.960 g/cc0.0347 lb/in³ISO 1183
Viscosity 330 cP
@Shear Rate 206 1/s,
Temperature 200 °C
330 cP
@Shear Rate 206 1/s,
Temperature 392 °F
ASTM D3835
Melt Flow 0.30 g/10 min
@Load 2.16 kg,
Temperature 230 °C
0.30 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  69
@Time 15.0 sec
69
@Time 0.00417 hour
Injection Molded; ISO 868
 71
@Time 5.00 sec
71
@Time 0.00139 hour
Injection Molded; ISO 868
 75
@Time 1.00 sec
75
@Time 0.000278 hour
Injection Molded; ISO 868
 71.9
@Treatment Temp. 125 °C,
Time 15.0 sec
71.9
@Treatment Temp. 257 °F,
Time 0.00417 hour
Change in Air, 168 hr; ISO 888
 72.1
@Treatment Temp. 110 °C,
Time 15.0 sec
72.1
@Treatment Temp. 230 °F,
Time 0.00417 hour
Change in Air, 1008 hr; ISO 888
 73.5
@Treatment Temp. 125 °C,
Time 5.00 sec
73.5
@Treatment Temp. 257 °F,
Time 0.00139 hour
Change in Air, 168 hr; ISO 888
 73.9
@Treatment Temp. 110 °C,
Time 5.00 sec
73.9
@Treatment Temp. 230 °F,
Time 0.00139 hour
Change in Air, 1008 hr; ISO 888
 76.7
@Treatment Temp. 110 °C,
Time 1.00 sec
76.7
@Treatment Temp. 230 °F,
Time 0.000278 hour
Change in Air, 1008 hr; ISO 888
 76.7
@Treatment Temp. 125 °C,
Time 1.00 sec
76.7
@Treatment Temp. 257 °F,
Time 0.000278 hour
Change in Air, 168 hr; ISO 888
Tensile Strength at Break 4.60 MPa667 psiFlow, Type 1, 20 in/min; ISO 37
 5.50 MPa798 psiAcross Flow, Type 1, 20 in/min; ISO 37
 4.62 MPa
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
670 psi
@Treatment Temp. 230 °F,
Time 1008 hour
Flow, Type 1, Change in Air; ISO 188
 4.70 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
682 psi
@Treatment Temp. 257 °F,
Time 168 hour
Flow, Type 1, Change in Air; ISO 188
 4.90 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
711 psi
@Treatment Temp. 257 °F,
Time 168 hour
Across Flow, Type 1, Change in Air; ISO 188
 5.61 MPa
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
814 psi
@Treatment Temp. 230 °F,
Time 1008 hour
Across Flow, Type 1, Change in Air; ISO 188
Tensile Stress at Strain  2.34 MPa
@Strain 100 %
339 psi
@Strain 100 %
Across Flow, Type 1, 20 in/min; ISO 37
 3.84 MPa
@Strain 100 %
557 psi
@Strain 100 %
Flow, Type 1, 20 in/min; ISO 37
 2.57 MPa
@Strain 100 %,
Treatment Temp. 110 °C
373 psi
@Strain 100 %,
Treatment Temp. 230 °F
Across Flow, Type 1, Change in Air, 1008 hr; ISO 188
 2.59 MPa
@Strain 100 %,
Treatment Temp. 125 °C
376 psi
@Strain 100 %,
Treatment Temp. 257 °F
Across Flow, Type 1, Change in Air, 6.61 in; ISO 188
 4.18 MPa
@Strain 100 %,
Treatment Temp. 110 °C
606 psi
@Strain 100 %,
Treatment Temp. 230 °F
Flow, Type 1, Change in Air, 1008 hr; ISO 188
 4.19 MPa
@Strain 100 %,
Treatment Temp. 125 °C
608 psi
@Strain 100 %,
Treatment Temp. 257 °F
Flow, Type 1, Change in Air, 168 hr; ISO 188
Elongation at Break 210 %210 %Flow, Type 1, 20 in/min; ISO 37
 450 %450 %Across Flow, Type 1, 20 in/min; ISO 37
 230 %
@Treatment Temp. 125 °C,
Time 605000 sec
230 %
@Treatment Temp. 257 °F,
Time 168 hour
Across Flow, Type 1, Change in Air; ISO 188
 246 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
246 %
@Treatment Temp. 230 °F,
Time 1008 hour
Flow, Type 1, Change in Air; ISO 188
 252 %
@Treatment Temp. 125 °C,
Time 605000 sec
252 %
@Treatment Temp. 257 °F,
Time 168 hour
Flow, Type 1, Change in Air; ISO 188
 474 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
474 %
@Treatment Temp. 230 °F,
Time 1008 hour
Across Flow, Type 1, Change in Air; ISO 188
Tear Strength 24.5 kN/m140 pliAcross Flow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
 24.5 kN/m140 pliFlow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
Compression Set  20 %
@Temperature 22.8 °C,
Time 79200 sec
20 %
@Temperature 73.0 °F,
Time 22.0 hour
Type 1; ISO 815
 32 %
@Temperature 70.0 °C,
Time 79200 sec
32 %
@Temperature 158 °F,
Time 22.0 hour
Type 1; ISO 815
 37 %
@Temperature 90.0 °C,
Time 252000 sec
37 %
@Temperature 194 °F,
Time 70.0 hour
Type 1; ISO 815
 49 %
@Temperature 125 °C,
Time 252000 sec
49 %
@Temperature 257 °F,
Time 70.0 hour
Type 1; ISO 815
 
Processing PropertiesMetricEnglishComments
Processing Temperature 190 - 230 °C374 - 446 °FInjection, Melt
Rear Barrel Temperature 173 - 213 °C344 - 416 °FInjection
Middle Barrel Temperature 179 - 219 °C354 - 426 °FInjection
Front Barrel Temperature 184 - 224 °C364 - 436 °FInjection
Nozzle Temperature 190 - 230 °C374 - 446 °FInjection
Zone 1 166 - 204 °C330 - 400 °FExtrusion
Zone 2 171 - 210 °C340 - 410 °FExtrusion
Zone 3 177 - 216 °C350 - 420 °FExtrusion
Zone 5 182 - 221 °C360 - 430 °FExtrusion
Die Temperature 190 - 227 °C374 - 440 °FExtrusion
Mold Temperature 35.0 - 60.0 °C95.0 - 140 °FInjection
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psiInjection
Back Pressure 0.172 - 0.862 MPa25.0 - 125 psiInjection
Cushion 0.381 - 2.54 cm0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpm30 - 100 rpmExtrusion
 50 - 120 rpm50 - 120 rpmInjection
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1135 / 237626

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.