MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Elix Polymers Elix™ E310 ABS Polymer
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Extruded

Material Notes: Extrusion grade, high impact resistance, high gloss surfaces. Automotive interior, Automotive exterior, Toys, Cosmetics packaging, Extruded sheets, Medical devices, Electroplating, Pipes, Covers, Smart cards.

Property data measured at 23°C and 50% RH.

Information provided by Elix Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 2.00 mm
0.0050 - 0.0070 in/in
@Thickness 0.0787 in
60 X 60 mm; ISO-294-4
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Thickness 2.00 mm
0.0050 - 0.0070 in/in
@Thickness 0.0787 in
60 X 60 mm; ISO-294-4
Melt Flow 7.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
7.0 g/10 min
@Load 22.0 lb,
Temperature 428 °F
cm³/10 min MVR; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 95.0 MPa13800 psiISO 2039-1
Tensile Strength, Yield 43.0 MPa6240 psi50 mm/min; ISO 527-1,2
Elongation at Break >= 15 %>= 15 %50 mm/min; acc. ISO 527-1,2
Elongation at Yield 2.5 %2.5 %50 mm/min; ISO 527-1,2
Tensile Modulus 2.20 GPa319 ksi1mm/min.; ISO 527-1,2
Flexural Strength 67.0 MPa9720 psi2mm/min; ISO 178
Flexural Modulus 2.20 GPa319 ksi2mm/min; ISO 178
Izod Impact, Notched (ISO)  11.0 kJ/m²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
 21.0 kJ/m²
@Temperature 23.0 °C
9.99 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Charpy Impact Unnotched  10.0 J/cm²
@Temperature -30.0 °C
47.6 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eU
 14.0 J/cm²
@Temperature 23.0 °C
66.6 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eU
Charpy Impact, Notched  1.40 J/cm²
@Temperature -30.0 °C
6.66 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eA
 2.20 J/cm²
@Temperature 23.0 °C
10.5 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+17 ohm-cm1.00e+17 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohm1.00e+15 ohmIEC 60093
Dielectric Constant  2.9
@Frequency 1e+6 Hz
2.9
@Frequency 1e+6 Hz
IEC 60250
 3.1
@Frequency 100 Hz
3.1
@Frequency 100 Hz
IEC 60250
Dielectric Strength 34.0 kV/mm864 kV/inIEC 60243-1
Dissipation Factor  0.0050
@Frequency 100 Hz
0.0050
@Frequency 100 Hz
IEC 60250
 0.0090
@Frequency 1e+6 Hz
0.0090
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 575 V575 Vsolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 100 °C212 °FISO 75-1,2
Deflection Temperature at 1.8 MPa (264 psi) 95.0 °C203 °FISO 75-1,2
Vicat Softening Point 100 °C212 °F50N 50°C/h; ISO 306
Glow Wire Flammability Index 700 °C
@Thickness 2.00 mm
1290 °F
@Thickness 0.0787 in
IEC 60695-2,12
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 °C464 °Finjection molding; ISO 294
Mold Temperature 70.0 °C158 °Finjection molding; ISO 294
Injection Velocity 240 mm/sec9.45 in/secinjection molding; ISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Trinseo Magnum™ 555 ABS
Elix Polymers ELIX ABS E401 Acrylonitrile Butadiene Styrene (ABS), Extrusion, Impact Grade
Chi Mei Polylac® PA-709 ABS
Elix Polymers Elix™ Ultra HH 4115 HI ABS Polymer
Elix Polymers Elix™ Ultra 4105 ABS Polymer

PELIX926 / 192520

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.