MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Advanced Ceramics ACL 1085 (C-795) Alumina
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: Information provided by Advanced Ceramics Limited (ACL)

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density >= 3.80 g/cc
Open Porosity 0.0 %
Grain Size 8.0 - 15 µm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell 45 N 79
Modulus of Elasticity 320 GPa
Shear Strength >= 300 MPa
@Temperature 20.0 °C
Cross Breaking Strength
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+17 ohm-cm
@Temperature 20.0 °C
Dielectric Constant 9.05
@Frequency 1e+9 Hz
 9.1
@Frequency 9.368e+9 Hz
 9.51
@Frequency 1e+7 Hz
Dielectric Strength 30.0 kV/mm
@Thickness 0.500 mm
Dissipation Factor <= 0.00010
@Frequency 1e+7 Hz
 <= 0.00010
@Frequency 1e+9 Hz
 <= 0.00030
@Frequency 9.368e+9 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.90 µm/m-°C
@Temperature 20.0 - 600 °C
 8.10 µm/m-°C
@Temperature 20.0 - 1000 °C
Thermal Conductivity >= 18.0 W/m-K
Maximum Service Temperature, Air 1000 °CTe Value Tk1
 1452 °CDeflection temperature; No load indicated.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Advanced Ceramics ALC 1082 (C-786) Alumina
Corundum, Aluminum Oxide, Alumina, 99.9%, Al2O3
Advanced Ceramics ALC 1081 (C-786) Alumina
Advanced Ceramics ACL 1091 (C-799) Alumina
Anderman Ceramics EA95 Sintered Alumina, 95%

CADVC02 / 466

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.