MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Covestro Texin® 990 Thermoplastic Polyurethanes (TPU) (Extended Aging Data)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Texin 990 resin is a polyether-based thermoplastic polyurethane with a Shore hardness of approximately 90A. It can be processed by injection molding, extrusion, or blow molding.

Properties / Applications Texin 990 resin offers outstanding abrasion resistance, impact strength, toughness, and flexibility. It also exhibits excellent inherent resistance to salt water stress cracking, and hydrolysis. Texin 990 natural color resin complies with FDA food-contact regulations 21 CFR 177.1680 (Polyurethane Resins) and 177.2600 (Rubber Articles Intended for Repeated Use), subject to the limitations of these and any other applicable regulations. In addition, Texin 990 natural color resin is listed under NSF standard 61 for use in potable water applications. Typical applications include belting, hose, seals and gaskets, tubing, cable and hose jackets, athletic soles, casters, film, extruded profiles and miscellaneous molded articles.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.13 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 90ASTM D2240
 86
@Time 252000 sec
Fuel C; ASTM D471
 86
@Time 605000 sec
Fuel C; ASTM D471
 86
@Time 1.21e+6 sec
Fuel C; ASTM D471
 87
@Time 1.81e+6 sec
Fuel C; ASTM D471
 90
@Time 605000 sec
Fuel A; ASTM D471
 90
@Time 1.81e+6 sec
Fuel A; ASTM D471
 91
@Time 252000 sec
Fuel A; ASTM D471
 92
@Time 1.21e+6 sec
Fuel A; ASTM D471
 84
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1; ASTM D471
 84
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #1; ASTM D471
 87
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #3; ASTM D471
 87
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #1; ASTM D471
 87
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #3; ASTM D471
 88
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3; ASTM D471
 88
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #3; ASTM D471
 88
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #1; ASTM D471
 90
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 90
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
 91
@Treatment Temp. 100 °C,
Time 605000 sec
Hot Air; ASTM D573
 92
@Treatment Temp. 100 °C,
Time 252000 sec
Hot Air; ASTM D573
Hardness, Shore D 36ASTM D2240
Tensile Strength at Break 41.4 MPaASTM D412
 29.808 MPa
@Time 1.81e+6 sec
Fuel C; ASTM D471
 29.808 MPa
@Time 252000 sec
Fuel C; ASTM D471
 30.222 MPa
@Time 1.21e+6 sec
Fuel C; ASTM D471
 31.05 MPa
@Time 605000 sec
Fuel C; ASTM D471
 44.298 MPa
@Time 1.21e+6 sec
Fuel A; ASTM D471
 45.98 MPa
@Time 605000 sec
Fuel A; ASTM D471
 46.358 MPa
@Time 252000 sec
Fuel A; ASTM D471
 49.266 MPa
@Time 1.81e+6 sec
Fuel A; ASTM D471
 37.042 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #1; ASTM D471
 37.26 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #1; ASTM D471
 37.674 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
 39.744 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #1; ASTM D471
 40.572 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #3; ASTM D471
 47.61 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #3; ASTM D471
 47.61 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1; ASTM D471
 48.024 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
Hot Air; ASTM D573
 50.508 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3; ASTM D471
 51.336 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
Hot Air; ASTM D573
 52.578 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 63.342 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #3; ASTM D471
Tensile Stress at Strain 6.20 MPa
@Strain 100 %
ASTM D412
 6.90 MPa
@Strain 50 %
ASTM D412
 7.65 MPa
@Strain 100 %
ASTM D412
 7.803 MPa
@Strain 100 %
ASTM Oil #3, 70; ASTM D471
 7.803 MPa
@Strain 100 %
ASTM Oil #3, 504; ASTM D471
 7.8795 MPa
@Strain 100 %
ASTM Oil #3, 168; ASTM D471
 7.8795 MPa
@Strain 100 %
ASTM Oil #3, 336; ASTM D471
 11.7 MPa
@Strain 300 %
ASTM D412
 14.21 MPa
@Strain 300 %
ASTM Oil #3, 504; ASTM D471
 14.5 MPa
@Strain 300 %
ASTM D412
 14.935 MPa
@Strain 300 %
ASTM Oil #3, 336; ASTM D471
 15.225 MPa
@Strain 300 %
ASTM Oil #3, 70; ASTM D471
 15.225 MPa
@Strain 300 %
ASTM Oil #3, 168; ASTM D471
 7.4205 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 504; ASTM D573
 7.803 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 70; ASTM D471
 7.956 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 168; ASTM D471
 8.0325 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 70; ASTM D573
 8.109 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 168; ASTM D573
 8.109 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 50; ASTM D471
 8.1855 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 336; ASTM D573
 8.262 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 336; ASTM D471
 11.02 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 504; ASTM D573
 13.195 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 336; ASTM D573
 14.355 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 70; ASTM D471
 14.645 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 168; ASTM D573
 14.645 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 336; ASTM D471
 14.935 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 70; ASTM D573
 14.935 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 50; ASTM D471
 16.53 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 168; ASTM D471
 5.8905 MPa
@Time 252000 sec,
Strain 100 %
Fuel C; ASTM D471
 6.12 MPa
@Strain 100 %,
Time 605000 sec
Fuel C; ASTM D471
 6.215 MPa
@Strain 100 %,
Time 1.21e+6 sec
Fuel C; ASTM D471
 6.426 MPa
@Strain 100 %,
Time 1.81e+6 sec
Fuel C; ASTM D471
 7.2675 MPa
@Time 252000 sec,
Strain 100 %
Fuel A; ASTM D471
 7.344 MPa
@Strain 100 %,
Time 1.21e+6 sec
Fuel A; ASTM D471
 7.5735 MPa
@Strain 100 %,
Time 605000 sec
Fuel A; ASTM D471
 7.5735 MPa
@Strain 100 %,
Time 1.81e+6 sec
Fuel A; ASTM D471
 8.342 MPa
@Strain 300 %,
Time 1.21e+6 sec
Fuel C; ASTM D471
 8.73 MPa
@Strain 300 %,
Time 1.81e+6 sec
Fuel C; ASTM D471
 9.312 MPa
@Time 605000 sec,
Strain 300 %
Fuel C; ASTM D471
 9.797 MPa
@Time 252000 sec,
Strain 300 %
Fuel C; ASTM D471
 9.894 MPa
@Strain 300 %,
Time 1.21e+6 sec
Fuel A; ASTM D471
 9.991 MPa
@Time 605000 sec,
Strain 300 %
Fuel A; ASTM D471
 10.088 MPa
@Strain 300 %,
Time 1.81e+6 sec
Fuel A; ASTM D471
 11.31 MPa
@Time 252000 sec,
Strain 300 %
Fuel C; ASTM D471
 11.745 MPa
@Time 605000 sec,
Strain 300 %
Fuel C; ASTM D471
 11.745 MPa
@Strain 300 %,
Time 1.21e+6 sec
Fuel C; ASTM D471
 11.89 MPa
@Strain 300 %,
Time 1.81e+6 sec
Fuel C; ASTM D471
 13.05 MPa
@Strain 300 %,
Time 1.21e+6 sec
Fuel A; ASTM D471
 13.63 MPa
@Time 252000 sec,
Strain 300 %
Fuel A; ASTM D471
 13.63 MPa
@Time 605000 sec,
Strain 300 %
Fuel A; ASTM D471
 14.065 MPa
@Strain 300 %,
Time 1.81e+6 sec
Fuel A; ASTM D471
Elongation at Break 520 %ASTM D412
 520 %
@Time 605000 sec
Fuel A; ASTM D471
 535.6 %
@Time 605000 sec
Fuel C; ASTM D471
 535.6 %
@Time 1.81e+6 sec
Fuel C; ASTM D471
 540.8 %
@Time 252000 sec
Fuel C; ASTM D471
 546 %
@Time 1.21e+6 sec
Fuel C; ASTM D471
 556.4 %
@Time 1.81e+6 sec
Fuel A; ASTM D471
 577.2 %
@Time 252000 sec
Fuel A; ASTM D471
 598 %
@Time 1.21e+6 sec
Fuel A; ASTM D471
 603.2 %
@Treatment Temp. 100 °C,
Time 252000 sec
Hot Air; ASTM D573
 624 %
@Treatment Temp. 100 °C,
Time 605000 sec
Hot Air; ASTM D573
 634.4 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3; ASTM D471
 665.6 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1; ASTM D471
 676 %
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #3; ASTM D471
 676 %
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #1; ASTM D471
 681.2 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #1; ASTM D471
 691.6 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #1; ASTM D471
 702 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #3; ASTM D471
 702 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #3; ASTM D471
 707.2 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 873.6 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
Flexural Modulus 41.4 MPaASTM D790
Compressive Strength 0.700 MPa2% Deflection; ASTM D 575
 1.70 MPa5% Deflection; ASTM D 575
 3.10 MPa10% Deflection; ASTM D 575
 4.50 MPa15% Deflection; ASTM D 575
 5.90 MPa20% Deflection; ASTM D 575
 7.20 MPa25% Deflection; ASTM D 575
 19.3 MPa50% Deflection; ASTM D 575
Resilience 32[%], Bayshore; ASTM D2632
 40[%], Bayshore; ASTM D2632
Tear Strength 87.66 kN/mDie C; ASTM D624
 96.3 kN/mDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 25
@Load 1.00 kg
[mg] Loss, H-18; ASTM D3489
 25
@Load 1.00 kg
[mg] Loss, H-18; ASTM D3489
Compression Set 13 %
@Temperature 23.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 13 %
@Temperature 23.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 20 %
@Temperature 23.0 °C,
Time 79200 sec
as molded; ASTM D395-B
 35 %
@Temperature 70.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 37 %
@Temperature 70.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 75 %
@Temperature 70.0 °C,
Time 79200 sec
as molded; ASTM D395-B
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 106 °CRate A; ASTM D1525
Brittleness Temperature >= -68.0 °FASTM D746
Glass Transition Temp, Tg -44.0 °C
 -40.0 °C
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 180 - 200 °CInjection
 182 - 199 °CExtrusion
 185 - 199 °CInjection
Middle Barrel Temperature 180 - 205 °CInjection
 182 - 204 °CInjection
 185 - 210 °CExtrusion
Front Barrel Temperature 180 - 210 °CInjection
 182 - 210 °CInjection
 185 - 215 °CExtrusion
Nozzle Temperature 185 - 215 °CInjection
 188 - 213 °CInjection
Zone 1 182 - 199 °CExtrusion
Zone 2 193 - 210 °CExtrusion
Zone 3 193 - 216 °CExtrusion
Die Temperature 190 - 215 °CExtrusion
Melt Temperature 193 - 210 °CInjection
 202 - 216 °CExtrusion
Mold Temperature 16.0 - 43.0 °CInjection
Injection Pressure 6000 - 14000 psiInjection
Hold Pressure 4000 - 8000 psiInjection
Back Pressure <= 200 psiInjection
 <= 800 psiInjection
Cushion <= 0.125 inInjection
 0.125 - 0.250 inInjection
 
Compliance PropertiesOriginal ValueComments
FDA Yes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PCOVEST0986a / 238169

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.