MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Daikin DAI-EL® G-575 Fluoroelastomer Terpolymer, Bisphenol Curable Grade, 70% Fluorine Content
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: Offers minimal compression set and excellent sealing. The terpolymer type is able to withstand polarized solvents to realize a wide range of application.

Features: Low permeability to gasoline and alcohol mixed fuel oil and good extrudability.

Information provided by Daikin Industries.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.91 g/cc
@Temperature 25.0 °C
1.91 g/cc
@Temperature 77.0 °F
Mooney Viscosity 36
@Temperature 121 °C
36
@Temperature 250 °F
ML 1+10
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7373Peak value, at 25°C
Tensile Strength at Break 12.9 MPa1870 psi
Tensile Stress at Strain 4.10 MPa
@Strain 100 %
595 psi
@Strain 100 %
Elongation at Break 290 %290 %
Tear Strength 19.8 kN/m113 pliat 25°C
Compression Set  24 %
@Temperature 100 °C
24 %
@Temperature 212 °F
70 hours
 28 %
@Temperature 175 °C
28 %
@Temperature 347 °F
70 hours
 44 %
@Temperature 200 °C
44 %
@Temperature 392 °F
70 hours
 32 %
@Temperature 25.0 °C,
Time 252000 sec
32 %
@Temperature 77.0 °F,
Time 70.0 hour
 
Thermal PropertiesMetricEnglishComments
Minimum Service Temperature, Air -11.0 °C12.2 °FTR test, TR10
 -9.00 °C15.8 °FGehman torsion test, T10
 -5.00 °C23.0 °FTR test, TR70
 -2.50 °C27.5 °FGehman torsion test, T2
Brittleness Temperature -18.0 °C-0.400 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 160 °C320 °FCure Measuring Temperature
Cure Time 6.70 min0.112 hourCurelastmeter
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 70 %70 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDAIK013 / 29305

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.