MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik 353 MA Tube and pipe, seamless
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Sandvik 353 MA is an austenitic chromium nickel steel alloyed with nitrogen and rare earth metals. The grade is characterized by:
  • High creep strength
  • Very good resistance to isothermal and cyclic oxidation
  • Very good resistance to combustion gases
  • Very good resistance to carburization
  • Good resistance to nitriding gases
  • Good structural stability at high temperatures
  • Good weldability
  • Maximum operating temperature is approx. 1175°C (2150°F)

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.90 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers <= 160
Tensile Strength, Ultimate >= 422 MPa
@Temperature 600 °C
 >= 437 MPa
@Temperature 500 °C
 >= 444 MPa
@Temperature 400 °C
 >= 470 MPa
@Temperature 300 °C
 >= 536 MPa
@Temperature 200 °C
 >= 650 MPa
@Temperature 100 °C
Tensile Strength, Yield >= 300 MPa
@Strain 0.2 %
 >= 340 MPa
@Strain 1 %
 >= 138 MPa
@Strain 0.2 %,
Temperature 600 °C
 >= 143 MPa
@Strain 0.2 %,
Temperature 500 °C
 >= 152 MPa
@Strain 0.2 %,
Temperature 400 °C
 >= 159 MPa
@Strain 1 %,
Temperature 600 °C
 >= 163 MPa
@Strain 1 %,
Temperature 500 °C
 >= 166 MPa
@Strain 0.2 %,
Temperature 300 °C
 >= 173 MPa
@Strain 1 %,
Temperature 400 °C
 >= 190 MPa
@Strain 1 %,
Temperature 300 °C
 >= 195 MPa
@Strain 0.2 %,
Temperature 200 °C
 >= 223 MPa
@Strain 1 %,
Temperature 200 °C
 >= 228 MPa
@Strain 0.2 %,
Temperature 100 °C
 >= 261 MPa
@Strain 1 %,
Temperature 100 °C
Elongation at Break >= 35 %
 >= 40 %Based on an original gauge length of 5.65 vS .
Creep Strength 1.80 MPa
@Temperature 1100 °C,
Time 3.60e+8 sec
1%
 2.30 MPa
@Temperature 1050 °C,
Time 3.60e+8 sec
1%
 2.70 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
1%
 3.00 MPa
@Temperature 1000 °C,
Time 3.60e+8 sec
1%
 3.50 MPa
@Temperature 1050 °C,
Time 3.60e+7 sec
1%
 3.90 MPa
@Temperature 950 °C,
Time 3.60e+8 sec
1%
 4.50 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
1%
 5.10 MPa
@Temperature 900 °C,
Time 3.60e+8 sec
1%
 6.00 MPa
@Temperature 950 °C,
Time 3.60e+7 sec
1%
 6.90 MPa
@Temperature 850 °C,
Time 3.60e+8 sec
1%
 8.00 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
1%
 9.70 MPa
@Temperature 800 °C,
Time 3.60e+8 sec
1%
 10.5 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
1%
 14.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
1%
 15.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
1%
 21.0 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
1%
 22.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
1%
 33.0 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
1%
 35.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
1%
 52.0 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
1%
 54.0 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
1%
 86.0 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
1%
 88.0 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
1%
 149 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
1%
Rupture Strength 2.90 MPa
@Temperature 1100 °C,
Time 3.60e+8 sec
 3.50 MPa
@Temperature 1050 °C,
Time 3.60e+8 sec
 4.50 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
 4.80 MPa
@Temperature 1000 °C,
Time 3.60e+8 sec
 6.00 MPa
@Temperature 1050 °C,
Time 3.60e+7 sec
 6.70 MPa
@Temperature 950 °C,
Time 3.60e+8 sec
 8.00 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
 10.0 MPa
@Temperature 900 °C,
Time 3.60e+8 sec
 11.0 MPa
@Temperature 950 °C,
Time 3.60e+7 sec
 14.0 MPa
@Temperature 850 °C,
Time 3.60e+8 sec
 15.0 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
 18.0 MPa
@Temperature 800 °C,
Time 3.60e+8 sec
 20.0 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
 25.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
 28.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
 52.0 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
 56.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
 63.0 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
 69.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
 80.0 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
 82.0 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
 127 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
 129 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
 206 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
Modulus of Elasticity 125 GPa
@Temperature 1100 °C
 130 GPa
@Temperature 1000 °C
 135 GPa
@Temperature 900 °C
 140 GPa
@Temperature 800 °C
 150 GPa
@Temperature 700 °C
 155 GPa
@Temperature 600 °C
 165 GPa
@Temperature 400 °C
 182 GPa
@Temperature 200 °C
 190 GPa
@Temperature 20.0 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000100 ohm-cm
@Temperature 20.0 °C
 0.0000107 ohm-cm
@Temperature 200 °C
 0.0000114 ohm-cm
@Temperature 400 °C
 0.0000120 ohm-cm
@Temperature 600 °C
 0.0000122 ohm-cm
@Temperature 700 °C
 0.0000125 ohm-cm
@Temperature 800 °C
 0.0000128 ohm-cm
@Temperature 900 °C
 0.0000130 ohm-cm
@Temperature 1000 °C
 0.0000132 ohm-cm
@Temperature 1100 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 15.5 µm/m-°C
@Temperature 20.0 - 100 °C
 15.5 µm/m-°C
@Temperature 20.0 - 200 °C
 16.5 µm/m-°C
@Temperature 20.0 - 400 °C
 17.0 µm/m-°C
@Temperature 20.0 - 600 °C
 17.0 µm/m-°C
@Temperature 20.0 - 700 °C
 17.5 µm/m-°C
@Temperature 20.0 - 800 °C
 18.0 µm/m-°C
@Temperature 20.0 - 900 °C
 18.0 µm/m-°C
@Temperature 20.0 - 1000 °C
 18.5 µm/m-°C
@Temperature 20.0 - 1100 °C
Specific Heat Capacity 0.480 J/g-°C
@Temperature 20.0 °C
 0.500 J/g-°C
@Temperature 100 °C
 0.530 J/g-°C
@Temperature 200 °C
 0.555 J/g-°C
@Temperature 300 °C
 0.575 J/g-°C
@Temperature 400 °C
 0.590 J/g-°C
@Temperature 500 °C
 0.610 J/g-°C
@Temperature 600 °C
 0.625 J/g-°C
@Temperature 700 °C
 0.640 J/g-°C
@Temperature 800 °C
 0.655 J/g-°C
@Temperature 900 °C
 0.665 J/g-°C
@Temperature 1000 °C
 0.680 J/g-°C
@Temperature 1100 °C
Thermal Conductivity 11.0 W/m-K
@Temperature 20.0 °C
 13.0 W/m-K
@Temperature 100 °C
 15.0 W/m-K
@Temperature 200 °C
 17.0 W/m-K
@Temperature 300 °C
 18.0 W/m-K
@Temperature 400 °C
 20.0 W/m-K
@Temperature 500 °C
 22.0 W/m-K
@Temperature 600 °C
 23.0 W/m-K
@Temperature 700 °C
 25.0 W/m-K
@Temperature 800 °C
 26.0 W/m-K
@Temperature 900 °C
 27.0 W/m-K
@Temperature 1000 °C
 29.0 W/m-K
@Temperature 1100 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.070 %
Cerium, Ce 0.050 %
Chromium, Cr 25 %
Manganese, Mn 1.5 %
Nickel, Ni 35 %
Nitrogen, N 0.16 %
Phosphorus, P <= 0.040 %
Silicon, Si 1.6 %
Sulfur, S <= 0.015 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sandvik 353 MA Seamless tube and pipe
MetalTek MTEK 25-35 Cast UNS N08705; Cast UNS J95705 Heat Resistant Stainless Steel
MetalTek HAYNES® HR120 Severe Corrosion and Heat Resistant Alloy
Haynes Stellite Alloy No. 27 cast, (UNS R30027) Superalloy
Carlson C 800H Nickel-Iron-Chromium Alloy

NSANDV5153 / 199717

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.