LG Chemical Lupox® GP2200 PBT+GF20%
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
;
Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled
Material Notes:
Description: Injection Molding, PBT+GF20%, General Purpose
Application: IT/OA, E&E, Automotive (Connector)
CAS No. 65997-17-3 and 24968-12-5
Information provided by LG Chemical
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.44
g/cc
1.44
g/cc
ASTM D792
Maximum Moisture Content
0.020
0.020
Injection Molding
Linear Mold Shrinkage, Flow
0.0040
-
0.011
cm/cm
@Thickness 3.20 mm
0.0040
-
0.011
in/in
@Thickness 0.126 in
ASTM D955
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
108
MPa
@Thickness 3.20 mm
15700
psi
@Thickness 0.126 in
50mm/min; ASTM D638
Elongation at Break
4.0 %
@Thickness 3.20 mm
4.0 %
@Thickness 0.126 in
5mm/min; ASTM D638
Flexural Yield Strength
157
MPa
@Thickness 3.20 mm
22800
psi
@Thickness 0.126 in
1.3mm/min; ASTM D790
Flexural Modulus
6.28
GPa
@Thickness 3.20 mm
910
ksi
@Thickness 0.126 in
1.3mm/min; ASTM D790
Izod Impact, Notched
0.588
J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
1.10
ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+16
ohm-cm
1.00e+16
ohm-cm
ASTM D257
Dielectric Strength
23.0
kV/mm
@Thickness 1.00 mm
584
kV/in
@Thickness 0.0394 in
ASTM D149
Arc Resistance
120
-
180
sec
120
-
180
sec
ASTM D495
Comparative Tracking Index
600
V
600
V
Solution A; IEC 60112
Hot Wire Ignition, HWI
7.0
-
15
sec
@Thickness >=1.50 mm
7.0
-
15
sec
@Thickness >=0.0591 in
15
-
30
sec
@Thickness >=3.00 mm
15
-
30
sec
@Thickness >=0.118 in
High Amp Arc Ignition, HAI
>=
120
arcs
@Thickness 1.50 mm
>=
120
arcs
@Thickness 0.0591 in
>=
120
arcs
@Thickness 3.00 mm
>=
120
arcs
@Thickness 0.118 in
Thermal Properties
Metric
English
Comments
Melting Point
225
°C
437
°F
@ Break; ASTM D3418
Deflection Temperature at 0.46 MPa (66 psi)
210
°C
@Thickness 6.40 mm
410
°F
@Thickness 0.252 in
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
200
°C
@Thickness 6.40 mm
392
°F
@Thickness 0.252 in
Unannealed; ASTM D648
UL RTI, Electrical
140
°C
@Thickness >=0.710 mm
284
°F
@Thickness >=0.0280 in
140
°C
@Thickness >=1.50 mm
284
°F
@Thickness >=0.0591 in
140
°C
@Thickness >=3.00 mm
284
°F
@Thickness >=0.118 in
UL RTI, Mechanical with Impact
120
°C
@Thickness >=0.710 mm
248
°F
@Thickness >=0.0280 in
120
°C
@Thickness >=1.50 mm
248
°F
@Thickness >=0.0591 in
120
°C
@Thickness >=3.00 mm
248
°F
@Thickness >=0.118 in
UL RTI, Mechanical without Impact
140
°C
@Thickness >=0.710 mm
284
°F
@Thickness >=0.0280 in
140
°C
@Thickness >=1.50 mm
284
°F
@Thickness >=0.0591 in
140
°C
@Thickness >=3.00 mm
284
°F
@Thickness >=0.118 in
Flammability, UL94
HB
@Thickness >=0.710 mm
HB
@Thickness >=0.0280 in
HB
@Thickness >=1.50 mm
HB
@Thickness >=0.0591 in
HB
@Thickness >=3.00 mm
HB
@Thickness >=0.118 in
Processing Properties
Metric
English
Comments
Rear Barrel Temperature
235
-
250
°C
455
-
482
°F
Injection Molding
Middle Barrel Temperature
240
-
250
°C
464
-
482
°F
Injection Molding
Front Barrel Temperature
245
-
255
°C
473
-
491
°F
Injection Molding
Nozzle Temperature
245
-
255
°C
473
-
491
°F
Injection Molding
Melt Temperature
245
-
255
°C
473
-
491
°F
Injection Molding
Mold Temperature
60.0
-
100
°C
140
-
212
°F
Injection Molding
Drying Temperature
120
°C
248
°F
Injection Molding
Dry Time
4.00
-
5.00
hour
4.00
-
5.00
hour
Injection Molding
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
LG Chemical LUCEL GC225 POM+GF25%, High Rigidity
LG Chemical Lupox® GP2300G PBT+GF30%
LG Chemical LI912 ASA
LG Chemical Lupox® GP2100 PBT+GF10%
LG Chemical HF350U ABS, High Flow
PLAY296 / 148306
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.