MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
3M Scotch-Weld™ 1300L Neoprene High Performance Rubber Gasket Adhesives
Categories: Polymer; Adhesive

Material Notes: 3M™ Scotch-Weld™ Neoprene High Performance Rubber ^& Gasket Adhesives 1300 is the most versatile of our rubber and gasket adhesives. They may be used to bond metal, wood, most plastics, and neoprene, reclaim, SBR, and butyl rubber. They have high immediate strength and excellent heat resistance. 3M Scotch-Weld Adhesive 1300L is a lower solids, lower viscosity version of 3M Scotch-Weld Adhesive 1300.

Information provided by 3M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Solids Content 26 - 33 %
Brookfield Viscosity 250 - 1000 cPRVF #2 sp @ 20 rpm @ 80°F
 
Mechanical PropertiesOriginal ValueComments
Shear Strength 85.0 psi
 85.0 psi
@Temperature 107 °C,
Time 1.81e+6 sec
Overlap, 1/8" Birch/Birch
 136 psi
@Temperature 82.0 °C,
Time 1.81e+6 sec
Overlap, 1/8" Birch/Birch
 195 psi
@Temperature -34.0 °C,
Time 1.81e+6 sec
Overlap, 1/8" Birch/Birch
 343 psi
@Temperature 75.0 °C,
Time 1.21e+6 sec
Overlap, 1/8" Birch/Birch
 549 psi
@Temperature 75.0 °C,
Time 1.81e+6 sec
Overlap, 1/8" Birch/Birch
Peel Strength 18.0 pli
@Temperature 24.0 °C,
Time 86400 sec
180°, Canvas/Steel
 26.0 pli
@Temperature 82.0 °C,
Time 1.81e+6 sec
180°, Canvas/Steel
 30.0 pli
@Temperature 24.0 °C,
Time 1.21e+6 sec
180°, Canvas/Steel
 32.5 pli
@Temperature 66.0 °C,
Time 1.81e+6 sec
180°, Canvas/Steel
 48.0 pli
@Temperature 24.0 °C,
Time 259000 sec
180°, Canvas/Steel
 49.0 pli
@Temperature -34.0 °C,
Time 1.81e+6 sec
180°, Canvas/Steel
 51.0 pli
@Temperature 24.0 °C,
Time 432000 sec
180°, Canvas/Steel
 52.0 pli
@Temperature 24.0 °C,
Time 605000 sec
180°, Canvas/Steel
 
Thermal PropertiesOriginal ValueComments
Flash Point -26.0 °CTCC
 
Descriptive Properties
AppearanceYellow
BasePolychloroprene

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
3M Scotch-Weld™ 10 Neoprene Contact Adhesive
3M Scotch-Weld™ 5 Neoprene Contact Adhesive
3M Scotch-Weld™ 2141 Neoprene Rubber & Gasket Adhesive
3M Scotch-Weld™ 1357-L Neoprene High Performance Contact Adhesive
3M Scotch-Weld™ 1357 Neoprene High Performance Contact Adhesive

PMM34115 / 168862

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.