MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
GEHR Plastics PPS-40GF Polyphenylene Sulfide, 40% Glass Fiber
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler

Material Notes: The linear polyphenylensulfide belongs to the semi-crystalline materials and offers a very high mechanical capacity, thermal and chemical resistance distinguished at the same time, high dimensional stability, and creep strength. The LOI belongs to the highest of polymers. By the reinforcement with glass polymers strength is achieved, which is comparable with light metal. PPS closes the gap between the technical synthetics and PEEK with its strength and economy.

Properties

  • very high strength and rigidity
  • high hardness
  • high thermostability
  • high dimensional stability
  • very high chemical resistance
  • very good insulating properties
  • high weather resistance
  • high resistance to hydrolysis
Applications include components in machine-making, pump parts, fan parts, impellers, parts in the fuel and automotive sector.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.65 g/ccISO 1183
Moisture Absorption at Equilibrium 0.010 %ISO 62
Water Absorption at Saturation 0.020 %ISO 62
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 100ISO 2039
Hardness, Shore D 90ISO 868
Ball Indentation Hardness 343 MPaISO 2039
Tensile Strength at Break 185 MPaISO 527
Tensile Strength, Yield 83.0 MPaISO 527
Elongation at Break 4.0 %ISO 527
Modulus of Elasticity 7.63 GPaISO 527
Flexural Strength 145 MPaISO 178
Charpy Impact Unnotched 26.0 kJ/m²ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 3.00e+13 ohm-cmIEC 60093
Surface Resistance >= 1.00e+13 ohmIEC 60093
Dielectric Constant 4.0
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 28.0 kV/mmIEC 60243-1
Dielectric Loss Index 0.0040
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 125 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.0 µm/m-°CISO 11359
Thermal Conductivity 0.250 W/m-K
@Temperature 20.0 °C
ISO 22007-4
Melting Point 280 °CDIN EN ISO 3146
Maximum Service Temperature, Air 230 °CUL 746B
Deflection Temperature at 1.8 MPa (264 psi) 260 °CISO 75
Glass Transition Temp, Tg 90.0 °CDIN EN ISO 3146
Flammability, UL94 V-0UL 94
 
Compliance PropertiesOriginal ValueComments
FDA YesPhysiological indifference
 
Descriptive Properties
Acid Resistanceyes
Aromatic Resistancelimited
Bondabilityyes
CKW Resistanceyes
Colorblack
Hydrocarbonate Resistanceyes
Hydroxide Resistancelimited
Ketone Resistancelimited
Physiological indifferenceyes, EEC
Resistance Against Hot Waterlimited
UV Stabilizationlimited

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler
Oxford Polymers PPS-40GF PPS, 40% Glass Fiber Reinforced
Ensinger TECATRON™ GF 40 Polyphenylene sulfide (PPS)
E-Polymers SEPAZ® K140HF 40% Glass Fiber Reinforced Low Flash, High Flow PPS Resin
RTP Company VLF 81307 Polyphenylene Sulfide (PPS), Long Glass Fiber

PGEHR036 / 79873

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.