MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Corundum, Aluminum Oxide, Alumina, 99.9%, Al2O3
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: Alpha aluminum oxide ('corundum' is the mineral name) is the stable form of pure aluminum oxide. Property values below are taken from literature and manufacturer sources. Variations are possible among various commercial grades.

Key Words: Alpha alumina, Al2O3, aluminum oxide, corundum, aluminium oxide
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 3.96 g/cc
Water Absorption 0.00 %
a Lattice Constant 4.7591 Å
c Lattice Constant 12.9894 Å
Formula Units/Cell (Z) 6
Molecular Weight 101.961 g/mol
Weibull Modulus >= 10
 
Chemical PropertiesOriginal ValueComments
Molar Volume 25.575 cc/mol
 
Mechanical PropertiesOriginal ValueComments
Hardness, Knoop 1700 - 2200
Hardness, Vickers 1365
Vickers Microhardness 2085
Hardness, Mohs 9.0
Abrasive Hardness 1000
Drilling Hardness 189000
Tensile Strength, Ultimate 300 MPa
Modulus of Elasticity 370 GPa
Flexural Strength 400 MPa
Compressive Strength 3000 MPa
 1900 MPa
@Temperature 1000 °C
Poissons Ratio 0.22
Fracture Toughness 4.00 MPa-m½
Shear Modulus 150 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+14 ohm-cm
 2.50e+6 ohm-cm
@Temperature 900 °C
Magnetic Susceptibility -0.0000370cm^3/mol
 -2.30e-7alternate reference
Dielectric Constant 9.9
Dielectric Strength 10.0 kV/mmWide Variation Between Grades
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 1093 J/g
Heat of Vaporization 19380 J/g
CTE, linear 0.600 µm/m-°C
@Temperature -173 °C
 3.30 µm/m-°C
@Temperature -73.0 °C
 5.50 µm/m-°C
@Temperature 25.0 °C
 7.10 µm/m-°C
@Temperature 127 °C
 7.50 µm/m-°C
@Temperature 227 °C
 7.90 µm/m-°C
@Temperature 327 °C
 8.50 µm/m-°C
@Temperature 527 °C
 9.10 µm/m-°C
@Temperature 727 °C
 9.60 µm/m-°C
@Temperature 927 °C
 10.1 µm/m-°C
@Temperature 1127 °C
 10.5 µm/m-°C
@Temperature 1327 °C
Specific Heat Capacity 0.850 J/g-°C
 0.126 J/g-°C
@Temperature -173 °C
 0.502 J/g-°C
@Temperature -73.0 °C
 0.753 J/g-°C
@Temperature 25.0 °C
 0.920 J/g-°C
@Temperature 127 °C
 1.046 J/g-°C
@Temperature 227 °C
 1.088 J/g-°C
@Temperature 327 °C
 1.172 J/g-°C
@Temperature 527 °C
 1.216 J/g-°C
@Temperature 727 °C
 1.238 J/g-°C
@Temperature 927 °C
 1.247 J/g-°C
@Temperature 1127 °C
 1.255 J/g-°C
@Temperature 1327 °C
Thermal Conductivity 30.0 W/m-K
 0.0251 cal cm/sec-cm²-°C
@Temperature 727 °C
 0.0310 cal cm/sec-cm²-°C
@Temperature 527 °C
 0.0451 cal cm/sec-cm²-°C
@Temperature 327 °C
 0.0579 cal cm/sec-cm²-°C
@Temperature 227 °C
 0.0773 cal cm/sec-cm²-°C
@Temperature 127 °C
 0.110 cal cm/sec-cm²-°C
@Temperature 25.0 °C
 0.196 cal cm/sec-cm²-°C
@Temperature -73.0 °C
 1.075 cal cm/sec-cm²-°C
@Temperature -173 °C
 6.30 W/m-K
@Temperature 800 °C
Melting Point 2054 °C
Boiling Point >= 3000 °C
Maximum Service Temperature, Air 1750 °CNo Load
Heat of Formation -1675.3 kJ/molCrystalline
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.761ω, Na
 1.769
@Wavelength 589.3 nm
η, Na
 
Component Elements PropertiesOriginal ValueComments
Al2O3 99.9 %
 
Descriptive Properties
ColorWhite
Crystal StructureRhombohedralCorundum

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum A357.0-T62, Cast
Overview - Alumina, 98%, Al2O3
Alumina, alpha Al2O3, 99.5%
Tungsten Carbide, WC
Aluminum, Al

BA1A / 134

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.