MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Eneos SIS5505 Styrene Isoprene Block Copolymer
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Applications: Adhesives

ENEOS has acquired the elastomer product lines from JSR Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.920 g/cc0.920 g/ccASTM D297
Brookfield Viscosity 1050 cP
@Temperature 25.0 °C
1050 cP
@Temperature 77.0 °F
25% in Toluene
Melt Flow  1.9 g/10 min
@Load 19.4 kg,
Temperature 21.2 °C
1.9 g/10 min
@Load 42.7 lb,
Temperature 70.2 °F
JIS K7210
 8.1 g/10 min
@Load 5.00 kg,
Temperature 200 °C
8.1 g/10 min
@Load 11.0 lb,
Temperature 392 °F
JIS K7210
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 3232JIS K7210
Tensile Strength 8.80 MPa1280 psiJIS K6251
Elongation at Break 1500 %1500 %JIS K6251
300% Modulus 0.500 MPa72.5 psiJIS K6251
 
Descriptive Properties
Composition[%], Styrene/Rubber
Content (%)50Diblock
Product formPellet

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PJSRC8175 / 295491

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.