MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ascend Performance Materials Starflam® 525H BK0771 PA66-GF25 FR
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass Fiber Filled, Flame Retardant

Material Notes: Starflam 525H BK0771 (formerly Vydyne® ECO525H BK0771) is a 25% glass reinforced PA66, heat stabilized, flame retardant that is halogen and red phosphorous free.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.40 g/cc0.0506 lb/in³DAM; ISO 1183
Linear Mold Shrinkage, Flow 0.0060 cm/cm
@Thickness 2.00 mm
0.0060 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cm
@Thickness 2.00 mm
0.0090 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 91.0 MPa13200 psi50% RH; ISO 527-2
 123 MPa17800 psiDAM; ISO 527-2
Elongation at Break 2.5 %2.5 %DAM; ISO 527-2
 3.0 %3.0 %50% RH; ISO 527-2
Tensile Modulus 7.00 GPa1020 ksi50% RH; ISO 527-2
 9.40 GPa1360 ksiDAM; ISO 527-2
Flexural Strength 129 MPa18700 psi50% RH; ISO 178
 197 MPa28600 psiDAM; ISO 178
Flexural Modulus 6.00 GPa870 ksi50% RH; ISO 178
 9.00 GPa1310 ksiDAM; ISO 178
Izod Impact, Notched (ISO)  7.30 kJ/m²
@Temperature -40.0 °C
3.47 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 180/1A
 7.40 kJ/m²
@Temperature -30.0 °C
3.52 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
 7.60 kJ/m²
@Temperature -30.0 °C
3.62 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 180/1A
 7.90 kJ/m²
@Temperature 23.0 °C
3.76 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 8.00 kJ/m²
@Temperature -40.0 °C
3.81 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 180/1A
 9.50 kJ/m²
@Temperature 23.0 °C
4.52 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1A
Charpy Impact Unnotched  5.20 J/cm²
@Temperature -40.0 °C
24.7 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 179/1eU
 5.20 J/cm²
@Temperature -40.0 °C
24.7 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eU
 5.20 J/cm²
@Temperature -30.0 °C
24.7 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eU
 5.50 J/cm²
@Temperature -30.0 °C
26.2 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eU
 5.90 J/cm²
@Temperature 23.0 °C
28.1 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
 6.00 J/cm²
@Temperature 23.0 °C
28.6 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eU
Charpy Impact, Notched  0.740 J/cm²
@Temperature -40.0 °C
3.52 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eA
 0.750 J/cm²
@Temperature -30.0 °C
3.57 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 0.760 J/cm²
@Temperature -40.0 °C
3.62 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 179/1eA
 0.790 J/cm²
@Temperature -30.0 °C
3.76 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eA
 0.870 J/cm²
@Temperature 23.0 °C
4.14 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength  19.0 kV/mm
@Thickness 1.00 mm
483 kV/in
@Thickness 0.0394 in
50% RH; IEC 60243
 31.0 kV/mm
@Thickness 1.00 mm
787 kV/in
@Thickness 0.0394 in
DAM; IEC 60243
Comparative Tracking Index 575 V
@Thickness 3.00 mm
575 V
@Thickness 0.118 in
IEC 60112
Hot Wire Ignition, HWI 60 - 120 sec60 - 120 secPLC 1; UL 746
 60 - 120 sec60 - 120 secPLC 1; UL 746
 >= 120 sec>= 120 secPLC 0; UL 746
 >= 120 sec>= 120 secPLC 0; UL 746
High Amp Arc Ignition, HAI >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
 
Thermal PropertiesMetricEnglishComments
Melting Point 260 °C500 °FDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 253 °C487 °FUnannealed; 50% RH; ISO 75-2/B
 255 °C491 °FUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 226 °C439 °FUnannealed; 50% RH; ISO 75-2/A
 237 °C459 °FUnannealed; DAM; ISO 75-2/A
UL RTI, Electrical  140 °C
@Thickness 0.200 mm
284 °F
@Thickness 0.00787 in
UL 746
 150 °C
@Thickness 0.400 mm
302 °F
@Thickness 0.0157 in
UL 746
 150 °C
@Thickness 0.750 mm
302 °F
@Thickness 0.0295 in
UL 746
 150 °C
@Thickness 1.50 mm
302 °F
@Thickness 0.0591 in
UL 746
 150 °C
@Thickness 3.00 mm
302 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical with Impact  110 °C
@Thickness 0.200 mm
230 °F
@Thickness 0.00787 in
UL 746
 115 °C
@Thickness 0.400 mm
239 °F
@Thickness 0.0157 in
UL 746
 130 °C
@Thickness 0.750 mm
266 °F
@Thickness 0.0295 in
UL 746
 140 °C
@Thickness 1.50 mm
284 °F
@Thickness 0.0591 in
UL 746
 140 °C
@Thickness 3.00 mm
284 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical without Impact  120 °C
@Thickness 0.200 mm
248 °F
@Thickness 0.00787 in
UL 746
 125 °C
@Thickness 0.400 mm
257 °F
@Thickness 0.0157 in
UL 746
 140 °C
@Thickness 0.750 mm
284 °F
@Thickness 0.0295 in
UL 746
 150 °C
@Thickness 1.50 mm
302 °F
@Thickness 0.0591 in
UL 746
 150 °C
@Thickness 3.00 mm
302 °F
@Thickness 0.118 in
UL 746
Flammability, UL94  V-0
@Thickness 0.200 mm
V-0
@Thickness 0.00787 in
 V-0
@Thickness 0.400 mm
V-0
@Thickness 0.0157 in
 V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
 5VA
@Thickness 1.50 mm
5VA
@Thickness 0.0591 in
 5VA
@Thickness 3.00 mm
5VA
@Thickness 0.118 in
Glow Wire Ignition Temperature 750 °C
@Thickness 0.400 mm
1380 °F
@Thickness 0.0157 in
IEC 60695-2-13
Glow Wire Flammability Index  960 °C
@Thickness 0.400 mm
1760 °F
@Thickness 0.0157 in
IEC 60695-2-12
 960 °C
@Thickness 0.750 mm
1760 °F
@Thickness 0.0295 in
IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
1760 °F
@Thickness 0.0591 in
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
1760 °F
@Thickness 0.118 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 275 - 300 °C527 - 572 °FInjection
Middle Barrel Temperature 275 - 300 °C527 - 572 °FInjection
Front Barrel Temperature 275 - 300 °C527 - 572 °FInjection
Melt Temperature 275 - 300 °C527 - 572 °FInjection
Mold Temperature 60.0 - 120 °C140 - 248 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hourInjection
 
Descriptive Properties
AdditiveFlame Retarding Agent
AppearanceBlack
FeaturesCorrosion Resistant
 Fast Molding Cycle
 Flame Retardant
 Good Dimensional Stability
 Good Processability
 Heat Aging Resistant
 High Flow
 High Strength
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PASCE9108 / 287559

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.