MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Magnesium
Magnesium Elektron - Service & Innovation in Magnesium

(Viewing data as-entered. Click here to return)
Magnesium Elektron Elektron® ZRE1 Magnesium Alloy, UNS M12330
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: ELEKTRON ZRE1 is a magnesium based alloy containing zinc, rare earths and zirconium. The alloy exhibits excellent casting characteristics with components being both pressure tight and weldable. It is creep resistant to 250°C.

Applications: The alloy is suitable for components operating at temperatures where creep resistance is required for low stressed complicated castings.

Information provided by Magnesium Elektron.

Key Words: ASTM B80 EZ33A-T5; AMS 4442; UNS M12330; BS 2L.126; BS2970 MAG6-TE; AIR 3380 ZRE1; AFNOR G-TR3Z2; DIN 1729 3.5103; Aircraft Number 3.6204; AECMA MG-C-91; ISO 2119 and 3115; MMPDS
Vendors: Magnesium Elektron is the world leader in high strength magnesium alloys in rolled, extruded and cast forms. Phone (303) 589-3189 or visit www.magnesium-elektron.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.80 g/cc
Bulk Density 0.0650 lb/in³Value supplied by MatWeb
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 50 - 60
Hardness, Vickers 55 - 70
Tensile Strength at Break >= 140 MPaMin Design Specification per BS 2L.126
 80.0 MPa
@Temperature 300 °C
 125 MPa
@Temperature 200 °C
 150 MPa
@Temperature 100 °C
 160 MPa
@Temperature 20.0 °C
Tensile Strength, Ultimate 154 MPa
@Temperature -196 °C
Tensile Strength, Yield >= 95.0 MPa
@Strain 0.2 %
Min Design Specification per BS 2L.126
 50.0 MPa
@Strain 0.2 %,
Temperature 300 °C
 75.0 MPa
@Strain 0.2 %,
Temperature 200 °C
 80.0 MPa
@Strain 0.2 %,
Temperature 100 °C
 110 MPa
@Strain 0.2 %,
Temperature 20.0 °C
Elongation at Break >= 3.0 %Min Design Specification per BS 2L.126
 0.50 %
@Temperature -196 °C
 3.0 %
@Temperature 22.0 °C
 15 %
@Temperature 100 °C
 25 %
@Temperature 200 °C
 50 %
@Temperature 300 °C
Creep Strength 15.0 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
0.1% creep
 20.0 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
0.2% creep
 24.0 MPa
@Temperature 250 °C,
Time 360000 sec
0.05% creep
 26.0 MPa
@Temperature 250 °C,
Time 360000 sec
0.1% creep
 26.0 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
0.5% creep
 28.0 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
1% creep
 31.0 MPa
@Temperature 250 °C,
Time 360000 sec
0.2% creep
 32.0 MPa
@Temperature 250 °C,
Time 36000 sec
0.05% creep
 35.0 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
0.05% creep
 35.0 MPa
@Temperature 250 °C,
Time 36000 sec
0.1% creep
 47.0 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
0.1% creep
 51.0 MPa
@Temperature 200 °C,
Time 360000 sec
0.05% creep
 55.0 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
0.2% creep
 65.0 MPa
@Temperature 200 °C,
Time 360000 sec
0.1% creep
Modulus of Elasticity 44.0 GPa
Compressive Yield Strength 85.0 - 120 MPa
@Strain 0.2 %
Compressive Strength 275 - 340 MPa
Ultimate Bearing Strength 395 MPa
Bearing Yield Strength 275 MPa
Poissons Ratio 0.33
Fatigue Strength 46.0 MPa
@# of Cycles 1.00e+7 ,
Temperature 300 °C
Rotating bend
 47.0 MPa
@# of Cycles 1.00e+6 ,
Temperature 300 °C
Rotating bend
 48.0 MPa
@# of Cycles 1.00e+7 ,
Temperature 250 °C
Rotating bend
 50.0 MPa
@# of Cycles 1.00e+6 ,
Temperature 250 °C
Rotating bend
 50.0 MPa
@# of Cycles 100000 ,
Temperature 300 °C
Rotating bend
 54.0 MPa
@# of Cycles 1.00e+7 ,
Temperature 200 °C
Rotating bend
 55.0 MPa
@# of Cycles 1.00e+6 ,
Temperature 200 °C
Rotating bend
 55.0 MPa
@# of Cycles 100000 ,
Temperature 250 °C
Rotating bend
 59.0 MPa
@# of Cycles 1.00e+7 ,
Temperature 150 °C
Rotating bend
 60.0 MPa
@# of Cycles 1.00e+6 ,
Temperature 150 °C
Rotating bend
 67.0 MPa
@# of Cycles 100000 ,
Temperature 200 °C
Rotating bend
 70.0 MPa
@# of Cycles 100000 ,
Temperature 150 °C
Rotating bend
 78.0 MPa
@# of Cycles 1.00e+7 ,
Temperature 20.0 °C
Rotating bend
 80.0 MPa
@# of Cycles 1.00e+6 ,
Temperature 20.0 °C
Rotating bend
 15.0 MPa
@# of Cycles 1.00e+7
"V" Notched
 20.0 MPa
@# of Cycles 1.00e+6
"V" Notched
 28.0 MPa
@# of Cycles 1.00e+7
"U" Notched
 30.0 MPa
@# of Cycles 1.00e+6
"U" Notched
 40.0 MPa
@# of Cycles 100000
"V" Notched
 60.0 MPa
@# of Cycles 100000
"U" Notched
 66.0 MPa
@# of Cycles 1.00e+7
Unnotched Rotating Bend, as cast
 68.0 MPa
@# of Cycles 1.00e+6
Unnotched Rotating Bend, as cast
 90.0 MPa
@# of Cycles 100000
Unnotched Rotating Bend, as cast
Shear Strength 138 MPa
Impact Test 0.700 - 2.00 JNotched Hounsfield
 6.10 - 7.40 JUnnotched Hounsfield
 0.500 J
@Temperature -196 °C
Unnotched Hounsfield
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000630 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 26.8 µm/m-°C
Specific Heat Capacity 1.04 J/g-°C
Thermal Conductivity 100 W/m-K
Melting Point 545 - 640 °C
Solidus 545 °C
Liquidus 640 °C
Maximum Service Temperature, Air 250 °Ccreep resistant
Shrinkage 1.5 %Pattern Makers Shrinkage Factor
 
Component Elements PropertiesOriginal ValueComments
Magnesium, Mg 92 - 95.1 %As Balance
Rare Earths 2.5 - 4.0 %
Zinc, Zn 2.0 - 3.0 %
Zirconium, Zr 0.40 - 1.0 %
 
Descriptive Properties
Corrosion rate270 mpyASTM B117 Salt spray test
Damping Index1.89

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Magnesium Elektron Elektron® AZ91E Magnesium Casting Alloy
Magnesium Elektron Elektron® ZK60A Magnesium Alloy, UNS M16600
Magnesium Elektron Elektron® RZ5 Magnesium Casting Alloy, UNS M16410
Magnesium AZ92A-T7, Cast
Magnesium Elektron Elektron® WE43B Magnesium Casting Alloy, UNS M18430

NMAGEL910 / 186925

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.