MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Chosun Refractories M55 Special High-Density Gunning Castable
Categories: Ceramic; Oxide; Magnesium Oxide

Material Notes:

Information provided by Chosun Refractories via Korea Institute of Ceramic Engineering and Technology (KICET).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density  2.69 g/cc
@Temperature 1500 °C,
Time 10800 sec
0.0972 lb/in³
@Temperature 2730 °F,
Time 3.00 hour
 2.79 g/cc
@Temperature 1000 °C,
Time 10800 sec
0.101 lb/in³
@Temperature 1830 °F,
Time 3.00 hour
 2.85 g/cc
@Temperature 110 °C,
Time 86400 sec
0.103 lb/in³
@Temperature 230 °F,
Time 24.0 hour
Porosity  16 %
@Temperature 110 °C,
Time 86400 sec
16 %
@Temperature 230 °F,
Time 24.0 hour
 21 %
@Temperature 1000 °C,
Time 10800 sec
21 %
@Temperature 1830 °F,
Time 3.00 hour
 22.5 %
@Temperature 1500 °C,
Time 10800 sec
22.5 %
@Temperature 2730 °F,
Time 3.00 hour
 
Mechanical PropertiesMetricEnglishComments
Modulus of Rupture  0.000981 GPa
@Temperature 1500 °C,
Time 10800 sec
0.142 ksi
@Temperature 2730 °F,
Time 3.00 hour
 0.0035316 GPa
@Temperature 1000 °C,
Time 10800 sec
0.51222 ksi
@Temperature 1830 °F,
Time 3.00 hour
 0.004905 GPa
@Temperature 110 °C,
Time 86400 sec
0.7114 ksi
@Temperature 230 °F,
Time 24.0 hour
 
Thermal PropertiesMetricEnglishComments
Shrinkage  -0.0300 %
@Temperature 110 °C,
Time 86400 sec
-0.0300 %
@Temperature 230 °F,
Time 24.0 hour
 0.15 %
@Temperature 1000 °C,
Time 10800 sec
0.15 %
@Temperature 1830 °F,
Time 3.00 hour
 1.5 %
@Temperature 1500 °C,
Time 10800 sec
1.5 %
@Temperature 2730 °F,
Time 3.00 hour
 
Component Elements PropertiesMetricEnglishComments
Al2O3 31 %31 %
MgO 54 %54 %
SiO2 15 %15 %
 
Descriptive Properties
Main ApplicationsSpecial furnace Main runner
Material Required for Estimating (kg/m3)2,800

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay HTM® 556 BMI
Owens Corning Glass Fiber Reinforced Polyester, Woven Roving (Lay-up), 50 wt.% glass
Beryllium, Be
Beryllium Copper, UNS C17200, TH01 Temper Strip

CCHOS236 / 124180

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.